专利摘要:
The invention relates to a nickel-based superalloy comprising, in percentages by weight, 4.0 to 6.0% of chromium, 0.4 to 0.8% of molybdenum, 2.5 to 3.5% of rhenium, 6 2 to 6.6% tungsten, 5.2 to 5.7% aluminum, 0.0 to 1.6% titanium, 6.0 to 9.9% tantalum, 0.0 to 0, 7% hafnium, 0.0 to 0.3% silicon, the balance being nickel and any impurities. The invention also relates to a monocrystalline blade (20A, 20B) comprising such an alloy and a turbomachine (10) comprising such a blade (20A, 20B).
公开号:FR3057880A1
申请号:FR1660337
申请日:2016-10-25
公开日:2018-04-27
发明作者:Jeremy Rame;Philippe Belaygue;Pierre Caron;Joel Delautre;Virginie Jaquet;Odile Lavigne
申请人:Office National dEtudes et de Recherches Aerospatiales ONERA;Safran Aircraft Engines SAS;Safran Helicopter Engines SAS;Safran SA;
IPC主号:
专利说明:

Holder (s): SAFRAN Société anonyme, SAFRAN AIRCRAFT ENGINES, NATIONAL OFFICE FOR AEROSPATIAL STUDIES AND RESEARCH Public establishment, SAFRAN HELICOPTER ENGINES.
Extension request (s)
Agent (s): CABINET BEAU DE LOMENIE.
FR 3 057 880 - A1
104 / NICKEL-BASED SUPERALLOY, MONOCRYSTALLINE VANE AND TURBOMACHINE.
The invention relates to a nickel-based superalloy comprising, in mass percentages, 4.0 to 6.0% of chromium, 0.4 to 0.8% of molybdenum, 2.5 to 3.5% of rhenium ,
6.2 to 6.6% tungsten, 5.2 to 5.7% aluminum, 0.0 to 1.6% titanium, 6.0 to 9.9% tantalum, 0.0 to 0 , 7% hafnium,
0.0 to 0.3% of silicon, the balance being made up of nickel and possible impurities.
The invention also relates to a monocrystalline blade (20A, 20B) comprising such an alloy and a turbomachine (10) comprising such a blade (20A, 20B).
BACKGROUND OF THE INVENTION The present disclosure relates to nickel-based superalloys for gas turbines, in particular for stationary vanes, also called distributors or rectifiers, or movable blades of a gas turbine, for example in the field of aeronautics.
It is known to use nickel-based superalloys for the manufacture of fixed or mobile monocrystalline blades of gas turbines for aircraft or helicopter engines.
The main advantages of these materials are that they combine both high creep resistance at high temperature as well as resistance to oxidation and corrosion.
Over time, nickel-based superalloys for monocrystalline blades have undergone significant changes in chemical composition, with the aim in particular of improving their creep properties at high temperature while retaining environmental resistance very aggressive in which these superalloys are used.
Furthermore, metal coatings suitable for these alloys have been developed in order to increase their resistance to the aggressive environment in which these alloys are used, in particular the resistance to oxidation and the resistance to corrosion. In addition, a ceramic coating of low thermal conductivity, fulfilling a thermal barrier function, can be added to reduce the temperature at the surface of the metal.
Typically, a complete protection system comprises at least two layers.
The first layer, also called sublayer or bonding layer, is directly deposited on the part to be protected in nickel-based superalloy, also called substrate, for example a blade. The deposition step is followed by a step of diffusion of the sublayer in the superalloy. The filing and dissemination can also be carried out in a single step.
The materials generally used to produce this undercoat include aluminoforming metal alloys of the MCrAlY type (M = Ni (nickle) or Co (cobalt) or a mixture of Ni and Co, Cr = chromium, Al = aluminum and Y = yttrium) or nickel aluminide alloys (Ni x Al y ), some also containing platinum (NixAlyPtz).
The second layer, generally called thermal barrier or "TBC" according to the acronym for "Thermal Barrier Coating", is a ceramic coating comprising for example yttria zirconia, also called "YSZ" according to the acronym English for "Yttria Stabilized Zirconia" or "YPSZ" according to the English acronym for "Yttria Partially Stabilized Zirconia" and having a porous structure. This layer can be deposited by various methods, such as evaporation under an electron beam (“EBPVD” according to the acronym for “Electron Beam Physical Vapor Deposition”), thermal spraying (“APS” according to English acronym for "Atmospheric Plasma Spraying"), "SPS" in accordance with the English acronym for "Suspension Plasma Spraying"), or any other process for obtaining a porous ceramic coating with low thermal conductivity.
Due to the use of these materials at high temperature, for example from 650 ° C to 1150 ° C, there are microscopic scale interdiffusion phenomena between the nickel-based superalloy of the substrate and the metal alloy of the underlay. These inter-diffusion phenomena, associated with the oxidation of the undercoat, modify in particular the chemical composition, the microstructure and consequently the mechanical properties of the undercoat from the manufacture of the coating, then during the use of dawn in the turbine. These inter-diffusion phenomena also modify the chemical composition, the microstructure and consequently the mechanical properties of the superalloy of the substrate. In superalloys very charged with refractory elements, in particular in rhenium, it can thus form in the superalloy under the sublayer a secondary reaction zone (ZRS) to a depth of several tens, even hundreds, of micrometers. The mechanical characteristics of this ZRS are significantly lower than those of the substrate superalloy. The formation of ZRS is undesirable since it leads to a significant reduction in the mechanical strength of the superalloy.
These changes in the bonding layer, associated with the stress fields linked to the growth of the alumina layer which forms in service on the surface of this bonding layer, also called "TGO" according to the acronym English for "Thermally Grown Oxide", and the differences in thermal expansion coefficients between the different layers, generate decohesions in the interfacial zone between the undercoat and the ceramic coating, which can lead to partial or total flaking of the ceramic coating. The metal part (superalloy substrate and metal sublayer) is then exposed and exposed directly to the combustion gases, which increases the risk of damaging the blade and therefore the gas turbine.
OBJECT AND SUMMARY OF THE INVENTION The present presentation aims to propose nickel-based superalloy compositions for the manufacture of monocrystalline components, showing mechanical characteristics at very high temperatures superior to those of existing alloys, and promoting resistance the flaking of the thermal barrier.
To this end, the present disclosure relates to a nickel-based superalloy comprising, in mass percentages, 4.0 to 6.0% of chromium, 0.4 to 0.8% of molybdenum, 2.5 to 3 , 5% rhenium, 6.2 to
6.6% tungsten, 5.2-5.7% aluminum, 0.0-1.6% titanium, 6-9.9% tantalum, 0-0.7% hafnium, 0, 0 to 0.3% silicon, the balance being made up of nickel and possible impurities.
This superalloy is intended for the manufacture of monocrystalline components of a gas turbine, such as fixed or mobile blades.
Thanks to this composition of the nickel-based superalloy (Ni), the creep resistance is improved compared to existing superalloys, in particular at temperatures up to 1200 ° C. and the adhesion of the thermal barrier. is reinforced compared to that observed on existing superalloys.
This alloy therefore has an improved creep resistance at high temperature. The lifetime of this alloy being thus long, this alloy also exhibits improved corrosion and oxidation resistance. This alloy can also have improved thermal fatigue resistance.
A monocrystalline part in a nickel-based superalloy is obtained by a solidification process directed under a thermal gradient in a lost-wax foundry. The nickel-based monocrystalline superalloy comprises an austenitic matrix of cubic structure with centered faces, solid solution based on nickel, called gamma phase (“γ”). This matrix contains precipitates of hardening gamma prime phase (“γ '”) of ordered cubic structure Ll 2 of Ni 3 AI type. The whole (matrix and precipitates) is therefore described as a γ / γ 'superalloy.
Furthermore, this composition of the nickel-based superalloy allows the use of a heat treatment which completely re-solves the γ 'phase precipitates and the γ / γ' eutectic phases which form during solidification. superalloy. It is thus possible to obtain a monocrystalline nickel-based superalloy containing precipitates γ 'of controlled size, preferably between 300 and 500 nanometers (nm), and free of eutectic phases γ / γ'.
The heat treatment also makes it possible to control the volume fraction of the γ 'phase precipitates present in the nickel-based monocrystalline superalloy. The percentage by volume of the γ 'phase precipitates can be greater than or equal to 50%, preferably greater than or equal to 60%, even more preferably equal to 70%.
The addition of tungsten (W), chromium (Cr), rhenium (Re) or molybdenum (Mo) mainly makes it possible to strengthen the austenitic matrix γ by hardening in solid solution.
The addition of aluminum (Al), titanium (Ti) or tantalum (Ta) promotes the precipitation of the hardening phase γ'-Νΐ 3 (ΑΙ, Ti, Ta).
Rhenium (Re) makes it possible to slow down the diffusion of chemical species within the superalloy and to limit the coalescence of the γ 'phase precipitates during service at high temperature, a phenomenon which results in a reduction in mechanical strength. Rhenium thus improves the creep resistance at high temperature of the nickel-based superalloy. However, too high a concentration of rhenium can cause the precipitation of intermetallic phases, for example phase o, phase P or phase μ, having a compact topology, also called phases TCP according to the acronym for “Topologically Close-Packed”, which have a negative effect on the mechanical properties of the superalloy. Too high a concentration of rhenium can also cause the formation of a secondary reaction zone in the superalloy under the sublayer, which has a negative effect on the mechanical properties of the superalloy.
The simultaneous addition of silicon (Si) and hafnium (Hf) improves the resistance to hot oxidation of nickel-based superalloys by increasing the adhesion of the alumina layer (AI 2 O 3 ) which forms on the surface of the superalloy at high temperature. This layer of alumina forms a passivation layer on the surface of the nickel-based superalloy and a barrier to the diffusion of oxygen from the outside to the inside of the nickel-based superalloy. However, it is possible to add hafnium without also adding silicon or, conversely, to add silicon without also adding hafnium and still improve the resistance to hot oxidation of the superalloy.
Furthermore, the addition of chromium or aluminum improves the resistance to oxidation and high temperature corrosion of the superalloy. In particular, chromium is essential for increasing the resistance to hot corrosion of nickel-based superalloys. Too high a chromium content, however, tends to reduce the solvent temperature of the y 'phase of the nickel-based superalloy, i.e. the temperature above which the y' phase is completely dissolved in the matrix y, which is undesirable. Also, the chromium concentration is between 4.0 to 6.0% by mass in order to maintain a high solvent temperature of the phase y 'of the nickel-based superalloy, for example greater than or equal to 1250 ° C. but also to avoid the formation of topologically compact phases in the matrix y highly saturated with elements of alloys such as rhenium, molybdenum or tungsten.
The addition of refractory elements, such as molybdenum, tungsten, rhenium or tantalum makes it possible to slow down the mechanisms controlling the creep of nickel-based superalloys and which depend on the diffusion of the chemical elements in the superalloy .
It will also be noted that the nickel-based superalloy does not include cobalt (Co), an element which has the effect of reducing the solvus temperature of the phase y '.
By impurities is meant chemical elements present in the metal in an unwanted manner and in small quantities, for example elements having a mass concentration less than or equal to 0.05%.
The term “nickel-based superalloys” is understood to mean superalloys in which the mass percentage of nickel is predominant. It is understood that nickel is therefore the element whose mass percentage in the alloy is the highest.
The superalloy can comprise, in mass percentages,
4.8 to 5.2% chromium, 0.4 to 0.8% molybdenum, 2.8 to 3.2% rhenium, 6.2 to 6.6% tungsten, 5.2 to 5, 7% aluminum, 0.8 to 1.2% titanium, 6.3 to 9.2% tantalum, 0.3 to 0.7% hafnium, 0.0 to 0.3% silicon, the remainder being made up of nickel and possible impurities.
The superalloy can comprise, in mass percentages,
4.8 to 5.2% chromium, 0.4 to 0.8% molybdenum, 2.8 to 3.2% rhenium, 6.2 to 6.6% tungsten, 5.2 to 5, 7% aluminum, 0.0 to 1.5% titanium, 6.3 to 6.7% tantalum, 0.3 to 0.7% hafnium, 0.0 to 0.3% silicon, the remainder being made up of nickel and possible impurities.
The superalloy can comprise, in mass percentages,
4.8 to 5.2% chromium, 0.4 to 0.8% molybdenum, 2.8 to 3.2% rhenium, 6.2 to 6.6% tungsten, 5.2 to 5, 7% aluminum, 0.0 to 0.5% titanium, 8.8 to 9.2% tantalum, 0.3 to 0.7% hafnium, 0.0 to 0.3% silicon, the remainder being made up of nickel and possible impurities.
The superalloy may comprise, in mass percentages, 5% chromium, 0.6% molybdenum, 3% rhenium, 6.4% tungsten, 5.5% aluminum, 1% titanium, 6 , 5% tantalum, 0.5% hafnium, 0.0 to 0.1% silicon, the balance being made up of nickel and possible impurities.
The superalloy can comprise, in mass percentages, 5% of chromium, 0.6% of molybdenum, 3% of rhenium, 6.4% of tungsten, 5.5% of aluminum, 9% of tantalum, 0 , 5% hafnium, 0.0 to 0.1% silicon, the balance consisting of nickel and possible impurities.
The present disclosure also relates to a monocrystalline blade for a turbomachine comprising a superalloy as defined above.
This blade therefore has an improved creep resistance at high temperature.
The blade can include a protective coating comprising a metal undercoat deposited on the superalloy and a ceramic thermal barrier deposited on the metal undercoat.
Thanks to the composition of the nickel-based superalloy, the inter-diffusion phenomena between the superalloy and the sublayer reduce, or even do not lead, to the formation of a secondary reaction zone in the superalloy.
Thanks to the composition of the nickel-based superalloy, the resistance to spalling of the thermal barrier on the blade is reinforced compared to the case of blades made of nickel-based superalloys of the prior art.
The metal sub-layer can be an alloy of the MCrAlY type or alloys of the nickel aluminide type.
The ceramic thermal barrier can be a material based on yttria zirconia or any other ceramic coating (based on zirconia) with low thermal conductivity.
The dawn may have a structure oriented in a crystallographic direction <001>.
This orientation generally gives optimal mechanical properties at dawn.
The present description also relates to a turbomachine comprising a blade as defined above.
Brief Description of the Drawings Other characteristics and advantages of the invention will emerge from the following description of embodiments of the invention, given by way of nonlimiting examples, with reference to the single appended figure, in which :
- Figure 1 is a schematic view in longitudinal section of a turbomachine.
Detailed description of the invention The nickel-based superalloys are intended for the manufacture of monocrystalline blades by a solidification process directed in a thermal gradient. The use of a monocrystalline seed or a grain selector at the start of solidification makes it possible to obtain this monocrystalline structure. The structure is oriented for example in a crystallographic direction <001> which is the orientation which generally confers the optimal mechanical properties on the superalloys.
The monocrystalline superalloys based on crude solidification nickel have a dendritic structure and consist of precipitates γ 'Nî 3 (AI, Ti, Ta) dispersed in a matrix γ of cubic structure with centered faces, solid solution based on nickel. These γ 'phase precipitates are distributed heterogeneously in the volume of the single crystal due to chemical segregation resulting from the solidification process. Furthermore, γ / γ 'eutectic phases are present in the interdendritic regions and constitute preferential sites for initiating cracks. In addition, the eutectic phases γ / γ 'are formed at the expense of fine precipitates (size less than a micrometer) of hardening phase γ'. These γ 'phase precipitates are the main source of hardening for nickel-based superalloys. Also, the presence of residual γ / γ 'eutectic phases does not make it possible to optimize the resistance to hot creep of the nickel-based superalloy.
It has indeed been shown that the mechanical properties of superalloys, in particular the creep resistance, were optimal when the precipitation of the precipitates γ 'was ordered, with a size ranging from 300 to 500 nm, and when all of the eutectic phases γ / γ 'was redissolved.
The superalloys based on crude solidification nickel are therefore heat treated to obtain the desired distribution of the different phases. The first heat treatment is a microstructure homogenization treatment which aims to dissolve the γ 'phase precipitates and the γ / γ' eutectic phases. This treatment is carried out at a temperature higher than the solvent temperature of the γ 'phase. Quenching is then carried out at the end of this first heat treatment to obtain a fine and homogeneous dispersion of the precipitates γ '. Tempering heat treatments are then carried out in two stages, at temperatures below the solvent temperature of the γ 'phase. During a first step, to enlarge the precipitates γ 'and obtain the desired size, then during a second step, to increase the volume fraction of this phase up to approximately 70%.
Examples Two monocrystalline nickel-based superalloys of the present description (Ex 1 and Ex 2) were studied and compared with three commercial monocrystalline superalloys CMSX-4 (Ex 3), AMI (Ex 4) and MC2 ( Ex 5). The chemical composition of each of the monocrystalline superalloys is given in Table 1. All these superalloys are nickel-based superalloys, that is to say that the complement to 100% of the concentrations presented in Table 1 consists of nickel and possible impurities.
Table 1
Co Cr Mo Re W Al Ti Your Hf Yes Ex 1 - 5 0.6 3 6.4 5.5 1 6.5 0.5 0.1 Ex 2 - 5 0.6 3 6.4 5.5 - 9 0.5 0.1 Ex 3 9 6.5 0.6 3 6 5.6 1 6.5 0.1 - Ex 4 6.5 7.5 2  - 5.5 5.3 1.2 8 0.1 - Ex 5 5 8 2 - 8 5 1.5 6 0.1 0.1
Creep resistance Table 2 presents the results of a creep resistance test under argon (Ar) at 1200 ° C. by applying a stress of 80 MPa, carried out on the superalloys Ex 1 to Ex 5. The creep resistance is quantified by the lifetime expressed in hours (h) of the specimen, that is to say the time elapsed between the start of the loading at 1200 ° C and the rupture of the test tube.
Table 2
Superalloys Service life (h) Ex 1 90 Ex 2 50 Ex 3 25
Ex 4 4 Ex 5 3
As can be seen, the superalloys Ex 1 and Ex 2 have a lifetime in creep at break, much greater than that of the comparison superalloys CMSX-4 (Ex 3), AMI (Ex 4) and MC2 ( Ex 5). The superalloys Ex 1 and Ex 2 can therefore either withstand operating stresses greater than those which the comparison superalloys can withstand, for comparable lifetimes, or show longer lifetimes under comparable stresses.
Resistance of the protective coating In order to study the compatibility of Ex 1 to Ex 5 superalloys with the coating (metallic undercoat and ceramic thermal barrier), tests of the resistance of the thermal barrier to cyclic oxidation were carried out. been made.
These tests, carried out in air, consist of the repetition of an elementary thermal cycle comprising a heating step up to 1100 ° C for ten minutes, followed by holding at 1100 ° C, the duration cumulative of these two steps being 1 h, and forced cooling for a dozen minutes to a temperature below 100 ° C.
The test is stopped when the test piece has a flaking of the ceramic thermal barrier on at least 20% of the surface of the test piece, that is to say when the ceramic thermal barrier is present on less than 80% of the surface of the test piece. This measurement can be carried out by image analysis.
The superalloys Ex 1 to Ex 5 were coated with a metallic underlay of the NiPtAI type and then with a ceramic thermal barrier of the yttria zirconia type deposited by EB-PVD. The yttria zirconia is of the 8YPSZ type which is a yttria zirconia comprising 8% by mass of yttrium oxide (Y 2 O 3 ).
The results of these tests are reported in Table 3 which shows the number of cycles at 1100 ° C performed on each test piece before the test is stopped.
The dispersion of the results of the various tests carried out on a type of superalloy is represented by the uncertainty expressed in number of cycles which can be added or subtracted from the value of the number of cycles in column 2 of Table 3. For each alloy , the test was carried out on at least three separate test pieces.
Table 3
Superalloys Number of cycles Uncertainty (number of cycles) Ex 1 4500 500 Ex 2 4300 500 Ex 3 2050 500 Ex 4 1450 250
It is noted that the test pieces having as compositions the compositions Ex 1 and Ex 2 can undergo a number of cycles between
1100 ° C and the temperature below 100 ° C in an oxidizing atmosphere much higher than the test pieces having as their compositions the compositions Ex 3 and Ex 4 before the thermal barrier flakes over more than 20% of the surface of the test tube.
The microstructure of the coated test pieces having the Ex 1 and Ex 2 compositions as their substrate was checked at the end of the thermal cycling tests between 1100 ° C. and the temperature below 100 ° C. Observations by optical microscopy demonstrate the absence of a secondary reaction zone in the superalloy substrate under the metal underlay of NiPtAI type.
In conclusion, the superalloys of the present presentation have, on the one hand, creep properties superior to those of the commercial alloys CMSX-4, AMI and MC2 (Ex 3 to Ex 5) at very high temperature (1200 ° C ). On the other hand, these superalloys make it possible to improve the lifetime of the thermal barrier. Finally, these alloys are not sensitive to the formation of a secondary reaction zone under the coating of the thermal barrier. These superalloys thus make it possible to increase the lifetime of the parts (turbine blades for example) at high temperature which are produced from these superalloys, in particular when these parts comprise a protective coating.
FIG. 1 represents, in section along a vertical plane passing through its main axis A, a turbofan engine 10. The turbofan engine 10 comprises, from upstream to downstream according to the circulation of the air flow, a blower 12, a low pressure compressor 14, a high pressure compressor 16, a combustion chamber 18, a high pressure turbine 20, and a low pressure turbine 22.
The high pressure turbine 20 comprises a plurality of movable vanes 20A rotating with the rotor and rectifiers 20B (fixed vanes) mounted on the stator. The stator of the turbine 20 comprises a plurality of stator rings 24 arranged opposite the movable blades 20A of the turbine 20.
These properties thus make these superalloys interesting candidates for the manufacture of monocrystalline parts intended for the hot parts of turbojets.
We can therefore manufacture a movable blade 20A or a rectifier 20B for a turbomachine comprising a superalloy as defined above.
It is also possible to manufacture a movable blade 20A or a rectifier 20B for a turbomachine comprising a superalloy as defined above covered with a protective coating comprising a metallic undercoat [0072] A turbomachine can in particular be a turbojet such as a turbofan 10. The turbomachine can also be a turbofan, a turboprop or a turboshaft.
Although the present description has been described with reference to a specific embodiment, it is obvious that various modifications and changes can be made to these examples without departing from the general scope of the invention as defined by the claims. In addition, individual features of the various embodiments discussed can be combined in additional embodiments. Therefore, the description and the drawings should be considered in an illustrative rather than restrictive sense.
权利要求:
Claims (10)
[1" id="c-fr-0001]
1. Nickel-based superalloy comprising, in mass percentages, 4.0 to 6.0% chromium, 0.4 to 0.8% molybdenum, 2.5 to 3.5% rhenium, 6.2 to 6.6% tungsten, 5.2-5.7% aluminum, 0.0-1.6% titanium, 6.0-9.9% tantalum, 0.0-0.7% hafnium, 0.0 to 0.3% silicon, the balance being made up of nickel and possible impurities.
[2" id="c-fr-0002]
2. Superalloy according to claim 1, comprising, in mass percentages, 4.8 to 5.2% of chromium, 0.4 to 0.8% of molybdenum, 2.8 to 3.2% of rhenium, 6.2 at 6.6% tungsten, 5.2 at
5.7% aluminum, 0.8 to 1.2% titanium, 6.3 to 9.2% tantalum, 0.3 to 0.7% hafnium, 0.0 to 0.3% silicon, the balance being made up of nickel and possible impurities.
[3" id="c-fr-0003]
3. Superalloy according to claim 1, comprising, in mass percentages, 4.8 to 5.2% of chromium, 0.4 to 0.8% of molybdenum, 2.8 to 3.2% of rhenium, 6.2 at 6.6% tungsten, 5.2 at
5.7% aluminum, 0.0 to 1.5% titanium, 6.3 to 6.7% tantalum, 0.3 to 0.7% hafnium, 0.0 to 0.3% silicon, the balance being made up of nickel and possible impurities.
[4" id="c-fr-0004]
4. Superalloy according to claim 1, comprising, in mass percentages, 4.8 to 5.2% of chromium, 0.4 to 0.8% of molybdenum, 2.8 to 3.2% of rhenium, 6.2 at 6.6% tungsten, 5.2 at
[5" id="c-fr-0005]
5.7% aluminum, 0.0 to 0.5% titanium, 8.8 to 9.2% tantalum, 0.3 to 0.7% hafnium, 0.0 to 0.3% silicon, the balance being made up of nickel and possible impurities.
5. Superalloy according to claim 1, comprising, in mass percentages, 5% chromium, 0.6% molybdenum, 3% rhenium, 6.4% tungsten, 5.5% aluminum, 1% titanium , 6.5% tantalum, 0.5% hafnium, 0.0 to 0.1% silicon, the balance consisting of nickel and possible impurities.
[6" id="c-fr-0006]
6. Superalloy according to claim 1, comprising, in mass percentages, 5% chromium, 0.6% molybdenum, 3% rhenium, 6.4% tungsten, 5.5% aluminum, 9% tantalum , 0.5% hafnium, 0.0 to 0.1% silicon, the balance consisting of nickel and possible impurities.
[7" id="c-fr-0007]
7. Monocrystalline blade (20A, 20B) for a turbomachine comprising a superalloy according to any one of claims 1 to
6.
[8" id="c-fr-0008]
8. Dawn (20A, 20B) according to claim 7, comprising a protective coating comprising a metallic undercoat deposited on the superalloy and a ceramic thermal barrier deposited on the metallic undercoat.
[9" id="c-fr-0009]
9. Dawn (20A, 20B) according to claim 7 or 8, having a structure oriented in a crystallographic direction <001>.
[10" id="c-fr-0010]
10. Turbomachine comprising a blade (20A, 20B) according to any one of claims 7 to 9.
1/1
类似技术:
公开号 | 公开日 | 专利标题
EP3532648B1|2020-11-25|Nickel based superalloy, single crystal blade and turbomachine
JP5362982B2|2013-12-11|Alloy compositions and articles containing the same
US8449262B2|2013-05-28|Nickel-based superalloys, turbine blades, and methods of improving or repairing turbine engine components
Guo et al.2019|Evaluation of microstructural degradation in a failed gas turbine blade due to overheating
US20140134353A1|2014-05-15|Nickel-based superalloys for use on turbine blades
FR3073527B1|2019-11-29|SUPERALLIAGE BASED ON NICKEL, MONOCRYSTALLINE AUBE AND TURBOMACHINE
EP3710611A1|2020-09-23|Nickel-based superalloy, single-crystal blade and turbomachine
EP3899083A1|2021-10-27|Turbine part made of superalloy comprising rhenium and/or ruthenium and associated manufacturing method
FR3072717B1|2019-10-11|SUPERALLIATION TURBINE PIECE COMPRISING RHENIUM AND METHOD OF MANUFACTURING THE SAME
FR3081883A1|2019-12-06|NICKEL-BASED SUPERALLOY, MONOCRYSTALLINE VANE AND TURBOMACHINE
FR3071272B1|2019-09-20|SUPERALLY TURBINE PIECE COMPRISING RHENIUM AND / OR RUTHENIUM AND PROCESS FOR PRODUCING THE SAME
FR3091709A1|2020-07-17|Nickel-based superalloy with high mechanical strength at high temperature
FR3113255A1|2022-02-11|Protection against oxidation or corrosion of a hollow superalloy part
WO2022029388A1|2022-02-10|Protection against oxidation or corrosion of a hollow part made of a superalloy
同族专利:
公开号 | 公开日
EP3532648A1|2019-09-04|
EP3532648B1|2020-11-25|
RU2019116001A3|2020-12-04|
FR3057880B1|2018-11-23|
RU2019116001A|2020-11-27|
ES2840099T3|2021-07-06|
JP2019537672A|2019-12-26|
WO2018078269A1|2018-05-03|
CA3041411A1|2018-05-03|
BR112019008164A2|2019-07-09|
US11220727B2|2022-01-11|
US20190330714A1|2019-10-31|
CN109963955A|2019-07-02|
RU2749981C2|2021-06-21|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
EP0971041A1|1998-07-07|2000-01-12|ONERA |Single crystal nickel-based superalloy with high solvus gamma prime phase|
WO2002022901A1|2000-09-15|2002-03-21|Cannon-Muskegon Corporation|Nickel-base superalloy for high temperature, high strain application|
EP1211336A1|2000-11-30|2002-06-05|ONERA |Nickel based superalloy for single crystal turbine blades of industrial turbines having a high resistance to hot corrosion|
WO2002070764A1|2001-03-01|2002-09-12|Cannon-Muskegon Corporation|Superalloy for single crystal turbine vanes|
EP1975261A1|2007-03-30|2008-10-01|Snecma|Thermal barrier deposited directly on monocrystalline superalloys|
DE3683091D1|1985-05-09|1992-02-06|United Technologies Corp|PROTECTIVE LAYERS FOR SUPER ALLOYS, WELL ADAPTED TO THE SUBSTRATES.|
US4719080A|1985-06-10|1988-01-12|United Technologies Corporation|Advanced high strength single crystal superalloy compositions|
JP2579316B2|1987-06-29|1997-02-05|大同特殊鋼株式会社|Single crystal Ni-base superalloy with excellent strength and corrosion resistance|
JP2546324B2|1988-03-14|1996-10-23|三菱マテリアル株式会社|Ni-based single crystal superalloy with excellent high temperature corrosion resistance|
US5435861A|1992-02-05|1995-07-25|Office National D'etudes Et De Recherches Aerospatiales|Nickel-based monocrystalline superalloy with improved oxidation resistance and method of production|
RU2149202C1|1996-04-16|2000-05-20|Сименс Акциенгезелльшафт|Article for direction of hot oxidizing gas|
US6095755A|1996-11-26|2000-08-01|United Technologies Corporation|Gas turbine engine airfoils having increased fatigue strength|
FR2780983B1|1998-07-09|2000-08-04|Snecma|SINGLE-CRYSTAL NICKEL-BASED SUPERALLOY WITH HIGHER TEMPERATURE RESISTANCE|
JP4230386B2|2004-03-08|2009-02-25|株式会社熊谷組|Tube unit|
KR20060045542A|2004-04-07|2006-05-17|유나이티드 테크놀로지스 코포레이션|Oxidation resistant superalloy and article|
JP5024797B2|2005-03-28|2012-09-12|独立行政法人物質・材料研究機構|Cobalt-free Ni-base superalloy|
US20100126014A1|2008-11-26|2010-05-27|General Electric Company|Repair method for tbc coated turbine components|
FR2941963B1|2009-02-10|2011-03-04|Snecma|METHOD FOR MANUFACTURING A THERMAL BARRIER COVERING A SUPERALLIATION METALLIC SUBSTRATE AND THERMOMECHANICAL PART RESULTING FROM THIS METHOD OF MANUFACTURE|
IT1394975B1|2009-07-29|2012-08-07|Nuovo Pignone Spa|NICKEL-BASED SUPERLEGA, MECHANICAL COMPONENT MADE WITH SUCH A SUPERLEGA, TURBOMACCHINA INCLUDING SUCH COMPONENT AND RELATIVE METHODS|
JP5660428B2|2010-04-20|2015-01-28|独立行政法人物質・材料研究機構|Heat-resistant coating material|FR3081883B1|2018-06-04|2020-08-21|Safran|NICKEL BASED SUPERALLY, MONOCRISTALLINE VANE AND TURBOMACHINE|
FR3084671B1|2018-07-31|2020-10-16|Safran|NICKEL-BASED SUPERALLY FOR MANUFACTURING A PART BY POWDER SHAPING|
FR3091709B1|2019-01-16|2021-01-22|Safran|High mechanical strength nickel-based superalloy at high temperature|
FR3091708B1|2019-01-16|2021-01-22|Safran|Low density nickel-based superalloy with high mechanical and environmental resistance at high temperature|
FR3092340B1|2019-01-31|2021-02-12|Safran|Nickel-based superalloy with high mechanical and environmental resistance at high temperature and low density|
CN110923638B|2019-11-29|2021-09-24|中国科学院金属研究所|Method for controlling stability of interface between thermal corrosion resistant single crystal alloy combustion engine blade and MCrAlY coating|
法律状态:
2017-09-20| PLFP| Fee payment|Year of fee payment: 2 |
2018-04-27| PLSC| Publication of the preliminary search report|Effective date: 20180427 |
2018-09-19| PLFP| Fee payment|Year of fee payment: 3 |
2019-09-19| PLFP| Fee payment|Year of fee payment: 4 |
2020-09-17| PLFP| Fee payment|Year of fee payment: 5 |
2021-09-22| PLFP| Fee payment|Year of fee payment: 6 |
优先权:
申请号 | 申请日 | 专利标题
FR1660337|2016-10-25|
FR1660337A|FR3057880B1|2016-10-25|2016-10-25|SUPERALLIAGE BASED ON NICKEL, MONOCRYSTALLINE AUBE AND TURBOMACHINE|FR1660337A| FR3057880B1|2016-10-25|2016-10-25|SUPERALLIAGE BASED ON NICKEL, MONOCRYSTALLINE AUBE AND TURBOMACHINE|
BR112019008164A| BR112019008164A2|2016-10-25|2017-10-24|nickel-based superalloy, monocrystalline shovel, and turbomachine.|
JP2019542807A| JP2019537672A|2016-10-25|2017-10-24|Nickel based superalloys, single crystal blades and turbomachines|
RU2019116001A| RU2749981C2|2016-10-25|2017-10-24|Nickel-based superalloy, single crystal blade and gas turbine engine|
US16/344,722| US11220727B2|2016-10-25|2017-10-24|Superalloy based on nickel, monocrystalline blade and turbomachine|
PCT/FR2017/052918| WO2018078269A1|2016-10-25|2017-10-24|Superalloy based on nickel, monocrystalline blade and turbomachine|
ES17797697T| ES2840099T3|2016-10-25|2017-10-24|Nickel-based superalloy, monocrystalline blade and turbomachine|
CA3041411A| CA3041411A1|2016-10-25|2017-10-24|Superalloy based on nickel, monocrystalline blade and turbomachine|
EP17797697.4A| EP3532648B1|2016-10-25|2017-10-24|Nickel based superalloy, single crystal blade and turbomachine|
CN201780066354.8A| CN109963955A|2016-10-25|2017-10-24|Nickel based super alloy, single crystal blade and turbine|
[返回顶部]