专利摘要:
A catalyst comprising at least one zeolite IZM-2 containing silicon atoms and aluminum atoms, at least one matrix and at least one metal of group VIII of the periodic table of elements, the zeolite having a ratio between number of moles of silicon and the number of moles of aluminum of between 60 and 150. Said catalyst is used in a process for isomerizing an aromatic filler comprising at least one compound containing eight carbon atoms per molecule.
公开号:FR3054454A1
申请号:FR1657146
申请日:2016-07-26
公开日:2018-02-02
发明作者:Christophe Bouchy
申请人:IFP Energies Nouvelles IFPEN;
IPC主号:
专利说明:

© Publication no .: 3,054,454 (to be used only for reproduction orders)
©) National registration number: 16 57146 ® FRENCH REPUBLIC
NATIONAL INSTITUTE OF INDUSTRIAL PROPERTY
COURBEVOIE
©) Int Cl 8 : B 01 J20 / 16 (2017.01), C 01 B 39/02, 39/46
A1 PATENT APPLICATION
©) Date of filing: 07.26.16. © Applicant (s): IFP ENERGIES NOUVELLES Etablis- (30) Priority: public education - FR. ©) Inventor (s): BOUCHY CHRISTOPHE. ©) Date of public availability of the request: 02.02.18 Bulletin 18/05. ©) List of documents cited in the report preliminary research: Refer to end of present booklet (© References to other national documents ©) Holder (s): IFP ENERGIES NOUVELLES Etablisse- related: public. ©) Extension request (s): @) Agent (s): IFP ENERGIES NOUVELLES.
CATALYST COMPRISING AN IZM-2 ZEOLITE HAVING AN OPTIMIZED IF / AL MOLAR RATIO FOR THE ISOMERIZATION OF C8 AROMATIC CUTS.
FR 3 054 454 - A1
A catalyst is described comprising at least one IZM-2 zeolite containing silicon atoms and aluminum atoms, at least one matrix and at least one metal from group VIII of the periodic table, the zeolite having a ratio between the number of moles of silicon and the number of moles of aluminum between 60 and 150. Said catalyst is used in a process for the isomerization of an aromatic charge comprising at least one compound with eight carbon atoms per molecule.
The present invention relates to a catalyst comprising a zeolite designated under the name IZM-2 of optimized silicon to aluminum molar ratio (Si / Al ratio, expressed in moles of silicon per mole of aluminum). The present invention also relates to a process for the isomerization of a C 8 aromatic cut using said isomerization catalyst.
State of the art
The sources of aromatics with eight carbon atoms mainly come from the reforming process (reformate) and steam cracking (pyrolysis essences). The distribution of aromatics with eight carbon atoms within these cuts is variable: generally from 10 to 30% of ethylbenzene with the three isomers of xylenes as complement: paraxylene, meta-xylene and ortho-xylene. Typically the distribution within this complement of xylenes is 50% in meta-xylene, 25% in ortho-xylene and 25% in paraxylene. Within this complement of xylenes, para-xylene is a particularly desirable isomer. Indeed the latter, via dimethyl terephthalate and terephthalic acid, allows the production of polyester fibers used for clothing and resins and films of polyethylene terephthalate (PET). It is thus desirable to maximize the production of para-xylene to the detriment of other aromatics with eight carbon atoms. This is achieved by implementing catalytic isomerization processes. After extraction of the para-xylene, the residual cut, rich in meta-xylene, ortho-xylene and ethylbenzene, is sent to a catalytic isomerization unit which gives a mixture of aromatics with eight carbon atoms in which the proportion of xylenes is close to thermodynamic equilibrium and the quantity of ethylbenzene reduced thanks to the conversion of ethylbenzene. This mixture is again sent to a para-xylene extraction unit and the residual cut sent to the isomerization unit. This creates a “C 8 aromatic loop” which maximizes the production of para-xylene (E. Guillon, P. Leflaive, Techniques de l'Ingénieur, J5920, V3). An isomerization unit can be used to isomerize the xylenes to para-xylene and convert ethylbenzene to benzene by the dealkylation reaction of ethylbenzene. In this case we speak of "dealkylating" isomerization of the cut. The residual cut can also be sent to an isomerization catalytic unit, to isomerize the xylenes to para-xylene and convert ethylbenzene to xylenes by the isomerization reaction of ethylbenzene. This is called “isomerizing” isomerization of the section. These industrial processes generally use heterogeneous catalysts implemented in a fixed bed and operating in the vapor phase under hydrogen pressure. These two types of process are distinguished by the operating conditions and by the formulation of the catalysts used (by their nature and / or their content in hydro-dehydrogenating function and / or in acid). The present invention is in the field of "isomerizing" isomerization.
In the case of "isomerizing" isomerization, the catalyst is of the bifunctional type and has both an acid function (generally provided by at least one zeolite) and a hydro-dehydrogenating function provided by a noble metal (generally platinum) . It has indeed been shown that the isomerization of ethylbenzene into xylenes involves a bifunctional type mechanism. Ethylbenzene is first hydrogenated to ethylcyclohexenes on the metal sites, these cycloolefin intermediates are then isomerized to dimethylcyclohexenes on the acid sites of Brcnsted. Finally the dimethylcyclohexenes are dehydrogenated into xylenes on the metal sites. The use of a strong hydro-dehydrogenating function such as platinum also induces the production of naphthenic cycles by hydrogenation of the corresponding aromatic cycles.
In addition to the desired isomerization reactions, it is desirable to limit side reactions of the type:
- dealkylation of ethylbenzene to benzene and ethylene;
- disproportionation of ethylbenzene to diethylbenzene and benzene, or xylenes to toluene and aromatics with 9 carbon atoms;
- transfer of alkyls between ethylbenzene and xylenes; and between the xylenes between them;
- opening of naphthenic cycles and cracking.
All of these reactions generate the production of less recoverable molecules, which are not recycled in the "C 8 aromatic loop" and are considered as net losses for the process. All molecules other than cyclic molecules with eight carbon atoms are thus considered to be net losses.
Isomerization reactions as well as side reactions are mainly catalyzed by the acid function. The properties of the zeolite (number and strength of Brcnsted acid sites, topology of the microporous network, etc.), acting as an acid function, thus have a direct impact on the properties of the bifunctional catalyst, and in particular its selectivity.
The catalysis of the isomerization of an aromatic C 8 cut into xylenes has thus been the subject of numerous patents relating to different zeolites. Among the zeolites used in isomerization of an aromatic C 8 cut, there is ZSM-5, used alone or in mixture with other zeolites, such as for example mordenite. These catalysts are described in particular in US patents 4,467,129 B and US 4,482,773 B. Other catalysts mainly based on mordenite have been described for example in patent FR 2,477,903 B. A catalyst has also been proposed. based on a EUO structural type zeolite (EP 923 987) or based on a MTW structural type zeolite (WO 2005 065380 A, WO 2010 000652 A, US 2014 0296601 A) or also based on a zeolite UZM8 in US patent 7,091,190 B.
These examples illustrate the continuous research carried out to develop ever more efficient catalysts for the isomerization of aromatic C 8 cuts, in particular by minimizing the production of net losses by the use of appropriate zeolites. For a given zeolitic structure, two factors are known to have an impact on its selectivity, and therefore on the selectivity of the catalyst. The first factor is the density of Brcnsted acid sites: the activity per acid site for bimolecular reactions such as the dismutation of ethylbenzene is proportional to the density of acid sites (M. Guisnet, Techniques de l'Ingénieur, j 1217 ). From this point of view it would therefore be desirable to use a zeolite having a low site density to minimize the parasitic reactions of disproportionation and transalkylation. The second factor is the strength of the acid sites: the dealkylation reaction of ethylbenzene to benzene involves the formation of unstable ethylcarbenium ions with a high energy barrier (P. Moreau, thesis at the University of Poitiers, 2005) and requires the presence of strong acid sites. This reaction is thus very sensitive to the strength of the acid sites of the zeolite. From this point of view it is therefore desirable to use a zeolite having few strong acid sites to minimize this type of parasitic reaction. However, for a given zeolitic structure, the strength of the acid sites is a function of their density: the acid sites are all the stronger as these are isolated, and therefore their density is low (C. Marcilly, acid catalysis- basic, volume 1, 2003). From this point of view it would therefore be desirable to use a zeolite having a high site density to minimize the parasitic dealkylation reactions. The minimization of the various parasitic reactions therefore requires contradictory requirements in terms of density of acid sites. In addition, ultimately the density of acid sites and their strength also dictate the overall activity of the zeolite.
As such, for a given zeolitic structure, it is necessary to identify the optimal range of acid site density allowing the best compromise between activity and selectivity to be obtained. The density of acid sites of a zeolite is, among other things, a function of the ratio between the number of moles of silicon and the number of moles of aluminum of said zeolite.
Recently, the applicant in its work has developed a new zeolite, the zeolite IZM-2 (FR 2 918 050 B), as well as its use in a catalyst for isomerization of a cut containing at least one aromatic compound with eight carbon atoms (FR 2 934 793 B). FR 2 918 050 B discloses an IZM-2 solid having a molar ratio of between 1 and 500. In the illustrative example of patent FR 2 934 793 B, only an IZM-2 solid having a Si / AI molar ratio of 53 is used for the isomerization of a cut containing at least one aromatic compound with eight carbon atoms.
Also, an objective of the present invention is to provide a new isomerization catalyst for the C 8 aromatic cut comprising an IZM-2 zeolite with an optimized Si / AI molar ratio, which has an X-ray diffraction diagram as given below. below, to limit the production of net losses.
Summary of the invention
J "-
The present invention relates to a catalyst comprising at least one IZM-2 zeolite, at least one matrix and at least one metal from group VIII of the periodic table, said catalyst being characterized in that the ratio between the number of moles of silicon and the number of moles of aluminum of the IZM-2 zeolite is between 60 and 150.
For the purposes of the present invention, the ratio between the number of moles of silicon and the number of moles of aluminum of the IZM-2 zeolite means the ratio of the number of moles of silicon divided by the number of moles of aluminum of the IZM-2 zeolite network.
The catalyst according to the invention is advantageously used in a process for isomerizing an aromatic cut comprising at least one aromatic compound containing eight carbon atoms per molecule, under the following operating conditions:
- a temperature of 300Ό to 50013,
- a partial hydrogen pressure of 0.3 to 1.5 MPa,
- a total pressure of 0.45 to 1.9 MPa, and
- a spatial feed speed, expressed in kilograms of feed introduced per kilogram of catalyst and per hour, from 0.25 to 30 h 1 .
It has been discovered, surprisingly, that the catalyst according to the invention comprising at least one matrix, at least one metal from group VIII of the periodic table of the elements, and at least the zeolite IZM-2 according to the invention whose ratio molar Si / AI is between 60 and 150, preferably between 60 and 110, very preferably between 60 and 100 and even more preferably between 60 and 95 leads to improved catalytic performance in terms of selectivity during a process for isomerizing an aromatic charge comprising at least one aromatic cut comprising at least one aromatic compound containing eight carbon atoms per molecule. Such a catalyst is significantly more selective than a catalyst comprising an IZM-2 zeolite whose Si / Al molar ratio is less than 60. This therefore results in a reduction in the production of the net losses for obtaining a given yield. in para-xylene when the isomerization process is carried out in the presence of the catalyst according to the invention.
Detailed description of the invention
The present invention relates to a catalyst comprising, and preferably consisting of, at least one IZM-2 zeolite containing silicon atoms and aluminum atoms, at least one matrix and at least one metal from group VIII of the periodic table. elements, said catalyst being characterized in that the ratio between the number of moles of silicon and the number of moles of aluminum of the IZM-2 zeolite is between 60 and 150.
Advantageously, the catalyst according to the invention is characterized in that it comprises an IZM-2 zeolite whose ratio of the number of moles of silicon divided by the number of moles of aluminum in the network of the zeolite is between 60 and 110 , very preferably between 60 and 100 and even more preferably between 60 and 95.
IZM-2 Zeolite
According to the invention, the catalyst comprises the zeolite IZM-2. The IZM-2 zeolite presents an X-ray diffraction diagram including at least the lines listed in Table 1. IZM-2 has a crystal structure.
Advantageously, the diffraction diagram is obtained by radiocrystallographic analysis by means of a diffractometer using the conventional method of powders with the radiation K a1 of copper (λ = 1.5406 Å). From the position of the diffraction peaks represented by the angle 2Θ, we calculate, by the Bragg relation, the reticular equidistances d hk i characteristic of the sample. The measurement error A (d hk i) on d hW is calculated using the Bragg relation as a function of the absolute error Δ (2θ) assigned to the measurement of 2Θ. An absolute error Δ (2θ) equal to ± 0.02 ° is commonly accepted. The relative intensity l re i assigned to each value of d hk is measured according to the height of the corresponding diffraction peak. The X-ray diffraction diagram of IZM-2 according to the invention comprises at least the lines with the values of d hk , given in table 1. In the column of d hk i, the mean values of the inter-reticular distances are indicated. in Angstroms (Â). Each of these values must be assigned the measurement error A (d hk i) between ± 0.6Â and ± 0.01 Â.
Table 1: average values of d ü kj and relative intensities measured on an X-ray diffraction diagram of the calcined IZM-2 crystallized solid.
2 theta (°) Ck, (Â) Irel 2 theta (°) ck (Â) Irel 5.07 17.43 ff 19.01 4.66 ff 7.36 12.01 FF 19.52 4.54 ff 7.67 11.52 FF 21.29 4.17 m 8.78 10.07 F 22.44 3.96 f 10.02 8.82 ff 23.10 3.85 mf 12.13 7.29 ff 23.57 3.77 f 14.76 6.00 ff 24.65 3.61 ff 15.31 5.78 ff 26.78 3.33 f 15.62 5.67 ff 29.33 3.04 ff 16.03 5.52 ff 33.06 2.71 ff 17.60 5.03 ff 36.82 2.44 ff 18.22 4.87 ff 44.54 2.03 ff
where FF = very strong; F = strong; m = medium; mf = medium weak; f = weak; ff = very weak.
The relative intensity l re i is given in relation to a relative intensity scale where a value of 100 is assigned to the most intense line of the X-ray diffraction diagram: ff <15; 15 <f <30; 30 <mf <50; 50 <m <65; 65 <F <85;FF> 85.
IZM-2 has a chemical composition expressed on an anhydrous basis, in terms of moles of oxides, defined by the following general formula: SiO 2 : a AI 2 O 3 : b M 2 / n O, in which M is at least an alkali metal and / or an alkaline earth metal of valence n. In said formula given above, a represents the number of moles of Al 2 O 3 and b represents the number of moles of M 2 / n O.
According to the invention, the number of moles of lattice aluminum per gram of IZM-2 zeolite is determined from the percentage (%) weight (wt) of aluminum in the zeolite and the percentage of tetaco and pentacoordinated aluminum present in the zeolite according to the formula:
n A i = [(% pdsAI) * (% RMNAI IV +% RMNAI V )] / [MM (AI) * 10000] with n A i: moles of lattice aluminum per gram of zeolite, in mole / gram, % pdsAI: percentage by weight of aluminum in the zeolite (dry mass), measured by inductively coupled plasma (ICP) on a SPECTRO ARCOS ICP-OES device from SPECTRO according to the ASTM D7260 method,
MM (AI): molar mass of aluminum, in grams / mole,% RMNAI IV : weight percentage of tetracoordinated aluminum in zeolite, measured by nuclear magnetic resonance of 27 AI,% RMNAI V : weight percentage of pentacoordined aluminum in the zeolite, measured by nuclear magnetic resonance of 27 AI.
The weight percentage of the tetracoordinated and pentacoordinated aluminum atoms present in the IZM-2 zeolite is determined by nuclear magnetic resonance of the solid of 27 AI. Aluminum NMR is indeed known to be used to identify and quantify the different coordination states of this nucleus (Physico-chemical analysis of industrial catalysts, J. Lynch, Editions Technip (2001) chap. 13, pages 290 and 291). The aluminum NMR spectrum of the IZM-2 zeolite can present three signals, a first being characteristic of the resonance of tetacoordinated aluminum atoms, a second being characteristic of pentacoordinated aluminum atoms and a third being characteristic of the resonance hexacoordinated aluminum atoms. The tetacoordinated aluminum atoms (denoted AI IV ) resonate at a chemical shift typically between +50 ppm and +70 ppm, the pentacoordinated aluminum atoms (denoted Al v ) resonate at a chemical shift typically between +20 ppm and +40 ppm and the hexacoordinated aluminum atoms (denoted AI VI ) resonate with a chemical shift typically between -20 ppm and +10 ppm. The weight percentage of the different aluminum species is quantified from the integration of the signals corresponding to each of these species. More specifically, the IZM-2 zeolite present in the catalyst according to the invention was analyzed by NMR-MAS of the solid 27 AI on a Brücker Avrom spectrometer of the 400 MHz Avance type using a 4 mm probe optimized for 27 AI. . The speed of rotation of the sample is close to 12 kHz. The aluminum atom is a quadrupole nucleus whose spin is equal to 5/2. In so-called selective analysis conditions, namely a low radio frequency field equal to 30 kHz, a low pulse angle equal to π / 2 and in the presence of a sample saturated with water, the NMR technique of rotation at the magic angle (MAS), denoted RMN-MAS, is a quantitative technique. The decomposition of each NMR-MAS spectrum provides direct access to the quantity of the various aluminum species, namely tetracoordinated aluminum atoms AI IV , pentacoordinated Al v and hexacoordinated AI VI . Each spectrum is calibrated in chemical displacement relative to a molar solution of aluminum nitrate for which the aluminum signal is at zero ppm. The signals characterizing the tetacoordinated aluminum atoms AI IV are typically integrated between +50 ppm and +70 ppm which corresponds to the area 1, the signals characterizing the pentacoordinated aluminum atoms Al v are typically integrated between +20 ppm and +40 ppm which corresponds to area 2 and the signals characterizing the hexacoordinated aluminum atoms AI VI are typically integrated between -20 ppm and +10 ppm which corresponds to area 3. The weight percentage of each aluminum species is calculated from the ratio between its area and the total area. For example, the weight percentage of hexacoordinated aluminum atoms AI VI (denoted% RMNAI VI ) is calculated as follows:
% RMNAI VI = (area 3) * 100 / (area 1 + area 2 + area 3)
Advantageously, the IZM-2 zeolite according to the invention has a weight percentage of hexacoordinated aluminum atoms AI VI (denoted% RMNAI VI ) of less than 50%, preferably less than 40%, and very preferably less than 30%.
The number of moles of silicon per gram of IZM-2 zeolite is determined from the percentage (%) weight (wt) in silicon of the zeolite according to the formula:
n S i = [(% wt%) / [MM (Si) * 100] with n Si : moles of silicon per gram of zeolite, in mole / gram,% wt%: percentage by weight of aluminum in the zeolite (dry mass) , measured by Fluorescence X by pearl assay on an AXIOS brand PANalytical device working at 125 mA and 32 kV,
MM (Si): molar mass of silicon, in grams / mole.
The ratio of the number of moles of silicon divided by the number of moles of lattice aluminum of the zeolite IZM-2 (Si / AI) is calculated according to the formula:
Si / AI = n Si / n A , with n S i / n A i: ratio of the number of moles of silicon divided by the number of moles of lattice aluminum, in mole / mole, ns ,: moles of silicon by gram of zeolite, in mole / gram,
Πλι: moles of lattice aluminum per gram of zeolite, in mole / gram.
The IZM-2 zeolite included in the catalyst according to the invention has an Si / AI molar ratio of between 60 and 150, preferably between 60 and 110, very preferably between 60 and 100 and even more preferably between 60 and 95.
In accordance with the invention, the desired Si / AI molar ratio for the IZM-2 zeolite can be obtained directly during the step for synthesizing the zeolite by adjusting the synthesis conditions and in particular the composition of the synthetic gel by controlling for example, the relative amounts of silicon and aluminum used in the synthesis gel.
A process for the preparation of the IZM-2 zeolite is taught in patent FR 2 918 050 B.
Advantageously, an aqueous mixture is reacted comprising at least one source of at least one oxide SiO 2 , optionally at least one source of at least one oxide AI 2 O 3 , optionally at least one source of at least one alkali and / or alkaline earth metal of valence n, and preferably at least one organic species R comprising two quaternary nitrogen atoms, the mixture preferably having the following molar composition:
SiO 2 / AI 2 O 3 : at least 2, preferably at least 20, more preferably from 60 to 600, H 2 O / SiO 2 : 1 to 100, preferably from 10 to 70,
R / SiO 2 : 0.02 to 2, preferably 0.05 to 0.5,
M 2 / n O / SiO 2 : 0 to 1, preferably 0.005 and 0.5, where M is one or more alkali and / or alkaline-earth metal (s) chosen from lithium, sodium, potassium, calcium, magnesium and the mixture of at least two of these metals, preferably M is sodium. Advantageously, the element R is 1,6bis (methylpiperidinium) hexane.
According to the invention, the Si / AI molar ratio of the IZM-2 zeolite can also be adjusted to the desired value by post-treatment methods of the IZM-2 zeolite obtained after synthesis. Such methods are known to those skilled in the art, and make it possible to carry out dealumination or desilication of the zeolite. Preferably, the Si / Al molar ratio of the IZM-2 zeolite forming part of the composition of the catalyst according to the invention is adjusted by an appropriate choice of the conditions of synthesis of said zeolite.
The IZM-2 zeolite present in the catalyst according to the invention is very advantageously in its acid form, that is to say in H + protonated form. In such a case, it is advantageous that the ratio of the number of moles of cation other than the proton per gram of IZM-2 zeolite divided by the number of moles of lattice aluminum per gram of IZM-2 zeolite is less than 0 , 9, preferably less than 0.6 and very preferably less than 0.3. To do this, the IZM-2 zeolite entering into the composition of the catalyst according to the invention can for example be exchanged by at least one treatment with a solution of at least one ammonium salt so as to obtain the ammonium form of the IZM-2 zeolite which once calcined leads to the acid form of said IZM-2 zeolite. This exchange stage can be carried out at any stage of the preparation of the catalyst, that is to say after the stage of preparation of the IZM-2 zeolite, after the stage of shaping the IZM-2 zeolite with a matrix, or even after the step of introducing the hydrodehydrogenating metal. Preferably the exchange step is carried out after the shaping step of the IZM-2 zeolite.
Matrix
According to the invention, the catalyst comprises at least one matrix. Said matrix can advantageously be amorphous or crystallized.
Preferably, said matrix is advantageously chosen from the group formed by alumina, silica, silica-alumina, clays, titanium oxide, boron oxide and zirconia, taken alone or as a mixture or else it is also possible to choose aluminates. Preferably, alumina is used as a matrix. Preferably, said matrix contains alumina in all its forms known to those skilled in the art, such as, for example, aluminas of the alpha, gamma, eta, delta type. Said aluminas differ in their specific surface and their pore volume. The mixture of the matrix and the IZM-2 zeolite formed forms the support for the catalyst.
Metallic phase
In accordance with the invention, the catalyst comprises at least one group VIII metal preferably chosen from iron, cobalt, nickel, ruthenium, rhodium, palladium, osmium, iridium and platinum, preferably chosen from the noble metals of group VIII, very preferably chosen from palladium and platinum and even more preferably platinum is chosen.
The dispersion of the group VIII metal (s), determined by chemisorption, for example by H 2 / O 2 titration or by chemisorption of carbon monoxide, is between 10% and 100%, preferably between 20% and 100% and even more preferably between 30% and 100%. The gross distribution coefficient of the group VIII metal (s), obtained from its profile determined by the Castaing microprobe, defined as the ratio of the group VIII metal (s) concentrations to the core of the grain relative to the edge of this same grain, is between 0.7 and 1.3, preferably between 0.8 and 1.2. The value of this ratio, close to 1, testifies to the homogeneity of the distribution of the group VIII metal (s) in the catalyst.
Said catalyst can advantageously comprise at least one additional metal chosen from the group formed by the metals of groups IIIA, IVA and VIIB of the periodic table of the elements and preferably chosen from gallium, indium, tin and rhenium. Said additional metal is preferably chosen from indium, tin and rhenium.
Catalyst preparation
The catalyst according to the invention can advantageously be prepared according to all the methods well known to those skilled in the art.
Fitness
Advantageously, the various constituents of the support or of the catalyst can be shaped by kneading stage to form a paste and then extrusion of the paste obtained, or else by mixing of powders then tableting, or else by any other known process of agglomeration of 'a powder containing alumina. The supports thus obtained can be in different shapes and dimensions. Preferably, the shaping is carried out by kneading and extrusion.
During the shaping of the support by kneading and then extrusion, said zeolite IZM-2 can be introduced during the dissolution or suspension of alumina compounds or alumina precursors such as bohemite, for example. Said IZM-2 zeolite can be, without being limiting, for example in the form of powder, ground powder, suspension, suspension having undergone a deagglomeration treatment. Thus, for example, said zeolite can advantageously be placed in an acidulated suspension or not at a concentration adjusted to the final content of IZM-2 targeted in the catalyst according to the invention. This suspension commonly called a slip is then mixed with the alumina compounds or alumina precursors.
Furthermore, the use of additives can advantageously be implemented to facilitate shaping and / or improve the final mechanical properties of the supports as is well known to those skilled in the art. By way of example of additives, mention may in particular be made of cellulose, carboxymethyl cellulose, carboxy ethyl cellulose, tall oil (tall oil), xanthan gums, surface-active agents, agents flocculants such as polyacrylamides, carbon black, starches, stearic acid, polyacrylic alcohol, polyvinyl alcohol, biopolymers, glucose, polyethylene glycols, etc.
Advantageously, water can be added or removed to adjust the viscosity of the paste to be extruded. This step can advantageously be carried out at any stage of the kneading step.
To adjust the solid content of the dough to be extruded in order to make it extrudable, it is also possible to add a predominantly solid compound and preferably an oxide or a hydrate. Preferably, a hydrate is used and even more preferably an aluminum hydrate. The loss on ignition of this hydrate is advantageously greater than 15%.
The extrusion of the dough from the kneading stage can advantageously be carried out by any conventional tool, commercially available. The paste resulting from the kneading is advantageously extruded through a die, for example using a piston or a single-screw or double extrusion screw. The extrusion can advantageously be carried out by any method known to those skilled in the art.
The catalyst supports according to the invention are generally in the form of cylindrical or multi-lobed extrudates such as bilobed, three-lobed, multi-lobed in straight or twisted shape, but can optionally be manufactured and used in the form of crushed powders, tablets, rings, balls and / or wheels. Preferably, the catalyst supports according to the invention have the form of spheres or extrudates. Advantageously, the support is in the form of extrudates with a diameter between 0.5 and 5 mm and more particularly between 0.7 and 2.5 mm. The shapes can be cylindrical (which can be hollow or not) and / or twisted and / or multilobed cylindrical (2, 3, 4 or 5 lobes for example) and / or rings. The multilobed form is advantageously used in a preferred manner.
Drying
The support thus obtained can then be subjected to a drying step. Said drying step is advantageously carried out by any technique known to a person skilled in the art.
Preferably, the drying is carried out under air flow. Said drying can also be carried out under the flow of any oxidizing, reducing or inert gas. Preferably, the drying is advantageously carried out at a temperature of between 50 and 180 ° C., preferably between 60 and 150 ° C. and very preferably between 80 and 130 ° C.
Calcination
Said support, optionally dried, then preferably undergoes a calcination step.
Said calcination step is advantageously carried out in the presence of molecular oxygen, for example by carrying out an air sweep, at a temperature advantageously greater than 200 ° C. and less than or equal to 1100 ° C. Said calcination step can advantageously be carried out in a crossed bed, in a licked bed or in a static atmosphere. For example, the oven used can be a rotary rotary oven or a vertical oven with radial traversed layers. Preferably, said calcination step is carried out between more than one hour at 200 ° C to less than one hour at 1100 ° C. The calcination can advantageously be carried out in the presence of water vapor and / or in the presence of acidic or basic vapor. For example, calcination can be carried out under partial pressure of ammonia.
Post-calcination treatments
Post-calcination treatments can optionally be carried out, so as to improve the properties of the support, in particular the textural properties.
Thus, the support of the catalyst used in the process according to the present invention can be subjected to a hydrothermal treatment in a confined atmosphere. Hydrothermal treatment in a confined atmosphere is understood to mean an autoclave treatment in the presence of water at a temperature above room temperature, preferably above 25 ° C., preferably above 30 ° C.
During this hydrothermal treatment, the support can advantageously be impregnated, before it is autoclaved (the autoclaving being carried out either in the vapor phase or in the liquid phase, this vapor or liquid phase of the autoclave being able to be acidic. or not). This impregnation, prior to autoclaving, can advantageously be acidic or not. This impregnation, prior to autoclaving, can advantageously be carried out dry or by immersion of the support in an acidic aqueous solution. By dry impregnation means contacting the support with a volume of solution less than or equal to the total pore volume of the support. Preferably, the impregnation is carried out dry. The autoclave is preferably an autoclave with a rotating basket such as that defined in patent application EP 0 387 109 A. The temperature during autoclaving can be between 100 and 250 ° C. for a period of time comprised between 30 minutes and 3 hours.
Deposition of the metallic phase
For the deposition of the metal from group VIII of the periodic table of the elements, all the deposition techniques known to those skilled in the art and all the precursors of such metals may be suitable. Deposition techniques can be used by dry impregnation or in excess of a solution containing the metal precursors, in the presence of competitors or not. The metal can be introduced at any stage of the preparation of the catalyst: on the IZM-2 zeolite and / or on the matrix, in particular before the shaping step, during the shaping step, or after the shaping step, on the catalyst support. Preferably, the metal is deposited after the shaping step.
The control of certain parameters implemented during the deposition, in particular the nature of the precursor of the metal (s) of group VIII used, makes it possible to direct the deposition of the said metal (s) ( ux) mainly on the matrix or on the zeolite.
Thus, to introduce the metal (s) (group) of group VIII, preferably platinum and / or palladium, mainly on the matrix, it is possible to use an anion exchange with hexachloroplatinic acid and / or hexachloropalladic acid, in the presence of a competing agent, for example hydrochloric acid, the deposit being generally followed by calcination, for example at a temperature between 350 and 550 ° C and for a period between 1 and 4 hours. With such precursors, the group VIII metal (s) is (are) deposited (s) mainly on the matrix and the said (s) metal (s) has (s) good dispersion and good macroscopic distribution across the grain of catalyst.
It is also possible to envisage depositing the group VIII metal (s), preferably platinum and / or palladium, by cation exchange so that the said metal (s) itself (in ) t deposited (s) mainly on the zeolite. Thus, in the case of platinum, the precursor can for example be chosen from:
- ammonia compounds such as platinum (II) tetramine salts of formula Pt (NH 3 ) 4 X 2 , platinum (IV) hexamine salts of formula Pt (NH 3 ) 6 X 4 ; the platinum (IV) halopentamine salts of formula (PtX (NH 3 ) 5 ) X 3 ; the platinum salts Ntetrahalodiamines of formula PtX 4 (NH 3 ) 2 ; and
- halogenated compounds of formula H (Pt (acac) 2 X);
X being a halogen chosen from the group formed by chlorine, fluorine, bromine and iodine, X being preferably chlorine, and acac representing the acetylacetonate group (of crude formula C 5 H 7 O 2 ), derived from acetylacetone. With such precursors, the metal (s) of group VIII is (are) deposited (s) mainly on the zeolite and the said (s) metal (s) has (s) good dispersion and good macroscopic distribution across the grain of catalyst.
In the case where the catalyst of the invention also contains at least one metal chosen from the metals of groups IIIA, IVA and VIIB, all the techniques for depositing such a metal known to those skilled in the art and all the precursors of such metals may be suitable.
The metal (s) of group VIII and that (s) of groups IIIA, IVA and VIIB can be added, either separately or simultaneously in at least one unitary step. When at least one group IIIA, IVA and VIIB metal is added separately, it is preferable that it is added after the group VIII metal.
The additional metal chosen from the metals of groups IIIA, IVA and VIIB can be introduced via compounds such as, for example, the chlorides, bromides and nitrates of the metals of groups IIIA, IVA and VIIB. For example in the case of indium, nitrate or chloride is advantageously used and in the case of rhenium, perrhenic acid is advantageously used. The additional metal chosen from the metals of groups IIIA, IVA and VIIB can also be introduced in the form of at least one organic compound chosen from the group consisting of the complexes of said metal, in particular the polyketonic complexes of the metal and the hydrocarbylmetals such than alkyls, cycloalkyls, aryls, alkylaryls and arylalkyls of metals. In the latter case, the introduction of the metal is advantageously carried out using a solution of the organometallic compound of said metal in an organic solvent. Organohalogenated metal compounds can also be used. As organic metal compounds, mention may be made in particular of tetrabutyltin, in the case of tin, and triphenylindium, in the case of indium.
If the additional metal chosen from the metals of groups IIIA, IVA and VIIB is introduced before the metal of group VIII, the metal compound IIIA, IVA and / or VIIB used is generally chosen from the group consisting of the halide, the nitrate , acetate, tartrate, carbonate and oxalate of the metal. The introduction is then advantageously carried out in aqueous solution. However, it can also be introduced using a solution of an organometallic compound of the metal, for example tetrabutyltin. In this case, before proceeding with the introduction of at least one group VIII metal, a calcination in air will be carried out.
In addition, intermediate treatments such as for example calcination and / or reduction can be applied between the successive deposits of the different metals.
Before its use in the process according to the invention, the catalyst is preferably reduced. This reduction step is advantageously carried out by treatment under hydrogen at a temperature between 150 ° C and 650 ° C and ui® total pressure between 0.1 and 25 MPa. For example, a reduction consists of a two-hour plateau at 150 ° C, then a temperature rise to 450 ° C at a speed of 1 ° C / min, then a two-hour plateau at 450 ° C; during this entire reduction step, the hydrogen flow rate is 1000 normal m 3 of hydrogen per ton catalyst and the total pressure kept constant at 0.2 MPa. Any ex situ reduction method can advantageously be considered. A prior reduction of the final catalyst ex situ, under a stream of hydrogen, can be implemented, for example at a temperature of 450 ° C to 600 ° C, for a period of 0.5 to 4 hours.
Said catalyst also advantageously comprises sulfur. In the case where the catalyst of the invention contains sulfur, this can be introduced at any stage of the preparation of the catalyst: before or after forming, and / or drying and / or calcination stage, before and / or after the introduction of the metal or metals mentioned above, or also by in situ and / or ex situ sulfurization before the catalytic reaction. In the case of in situ sulfurization, the reduction, if the catalyst has not been previously reduced, takes place before the sulfurization. In the case of ex situ sulfurization, the reduction is also carried out followed by the sulfurization. The sulfurization is preferably carried out in the presence of hydrogen using any sulphurizing agent well known to the skilled person, such as for example dimethyl sulphide or hydrogen sulphide.
The catalysts according to the invention come in different forms and dimensions. They are generally used in the form of cylindrical and / or multi-lobed extrudates such as two-lobed, three-lobed, multi-lobed straight and / or twisted, but can optionally be manufactured and used in the form of crushed powders, tablets, rings, balls and / or wheels. Preferably, the catalysts used in the process according to the invention have the form of spheres or extrudates. Advantageously, the catalyst is in the form of extrudates with a diameter of between 0.5 and 5 mm and more particularly between 0.7 and 2.5 mm. The shapes can be cylindrical (which can be hollow or not) and / or twisted and / or multilobed cylindrical (2, 3, 4 or 5 lobes for example) and / or rings. The multilobed form is advantageously used in a preferred manner. The deposition of the metal does not change the shape of the support.
Said catalyst according to the invention more particularly comprises, and preferably consists of:
from 1 to 90%, preferably from 3 to 80% and even more preferably from 4 to 60% by weight of the IZM-2 zeolite according to the invention,
- from 0.01 to 4%, preferably from 0.05 to 2% by weight of at least one metal from group VIII of the periodic table of the elements, preferably platinum,
- optionally from 0.01 to 2%, preferably from 0.05 to 1% by weight of at least one additional metal chosen from the group formed by the metals of groups IIIA, IVA and VIIB,
- optionally a sulfur content, preferably such that the ratio of the number of moles of sulfur to the number of moles of group VIII metal (s) is between 0.3 and 3,
- at least one matrix, preferably alumina, ensuring the complement to 100% in the catalyst.
The isomerization process
The present invention also relates to a process for isomerizing a cut containing at least one aromatic compound with eight carbon atoms per molecule, said process comprising bringing said aromatic cut into contact with at least said catalyst according to the invention present in a catalytic reactor.
Said aromatic moiety containing at least one aromatic compound having eight carbon atoms per molecule comprises in particular as aromatic compound having eight carbon atoms per molecule either only a mixture of xylenes, or only ethylbenzene, or a mixture of xylene (s ) and ethylbenzene.
Said isomerization process is generally carried out according to the following operating conditions:
- a temperature from 300 ° C to 500 ° C, preferably from 320 ° C to 450 ° C and even more preferably from 340 ° C to 430 ° C;
a partial pressure of hydrogen of 0.3 to 1.5 MPa, preferably of 0.4 and 1.2 MPa and more preferably of 0.7 to 1.2 MPa;
- a total pressure from 0.45 to 1.9 MPa, preferably from 0.6 to 1.5 MPa; and
- a spatial feed speed, expressed in kilograms of feed introduced per kilogram of catalyst and per hour, from 0.25 to 30 h 1 , preferably from 1 to 10 h 1 and more preferably from 2 to 6 h 1 .
The following examples illustrate the invention without, however, limiting its scope.
Examples
Example 1 (not in accordance with the invention): preparation of the isomerization catalyst A
Catalyst A is a catalyst comprising an IZM-2 zeolite, platinum, and an alumina matrix. This zeolite IZM-2 was synthesized in accordance with the teaching of the patent FR 2 918 050 B. A colloidal suspension of silica known under the commercial term Ludox HS-40 marketed by Aldrich, is incorporated into a solution composed of soda (Prolabo) , structuring dibromide of 1,6bis (methylpiperidinium) hexane, aluminum hydroxide (Aldrich) and deionized water. The molar composition of the mixture is as follows: 1 SiO 2 ; 0.0033 AI 2 O 3 ; 0.1666 Na 2 O; 0.1666 1.6bis (methylpiperidinium) hexane;
33.3333 H 2 O. The mixture is stirred vigorously for half an hour. The mixture is then transferred, after homogenization, to a PARR type autoclave. The autoclave is heated for 5 days at 170 ° C. with stirring in a spit (30 rpm). The product obtained is filtered, washed with deionized water to reach a neutral pH and then dried overnight at 100 ° C in an oven. The solid is then introduced into a muffle furnace to be calcined there in order to remove the structuring agent. The calcination cycle includes a temperature rise up to 200 ° C, a plateau at this temperature of two hours, a temperature rise up to 550 ° C followed by an eight hour plateau at this temperature and finally a return at room temperature. The temperature rises are carried out with a ramp of 2 ° C / min. The solid thus obtained is then placed under reflux for 2 hours in an aqueous solution of ammonium nitrate (10 ml of solution per gram of solid, concentration of ammonium nitrate of 3 M) in order to exchange the sodium alkaline cations by ammonium ions. This refluxing step is carried out four times with a fresh solution of ammonium nitrate, then the solid is filtered, washed with deionized water and dried in an oven overnight at 100 ° C. Finally, to obtain the zeolite in its acid form (protonated H + ) a calcination step is carried out at 550 ° C for ten hours (temperature rise ramp of 2 ° C / min) in a bed crossed with dry air (2 normal liters per hour and per gram of solid). The solid thus obtained was analyzed by X-ray diffraction and identified as being constituted by the zeolite IZM-2. The zeolite, named IZM-2A, is used for the preparation of the catalyst. Characterizations using 27 AI NMR, X-ray fluorescence and ICP methods give access to the following results for ΙΊΖΜ2 A:
- weight percentage of hexacoordinated aluminum atoms AI VI : 9%,
- ratio of the number of moles of silicon divided by the number of moles of lattice aluminum, in mole / mole, Si / AI: 113,
- ratio of the number of moles of sodium divided by the number of moles of lattice aluminum, in mole / mole, Na / Al: 0.22.
Platinum is deposited on a gamma alumina matrix by an excess impregnation method. Gamma alumina supplied by the company Axens (GOD200) is in the form of beads. First, the beads are saturated by filling the pore volume with distilled water (dropwise addition) then wetting for typically 30 minutes. The alumina is then acidified with an aqueous acid solution up to 5% by weight in chlorine relative to the mass of dry alumina (4 ml of solution per gram of solid) and the mixture is left stirring for one hour on stirring table then the solution is drawn off. An excess impregnation is then carried out with an aqueous solution of hexachloroplatinic acid up to 2% by weight of platinum relative to the mass of dry alumina (4 ml of solution per gram of solid) and then left to stir on a table. stirring for 24 hours, then the solution is drawn off and the solid is rinsed with twice the volume of exchange of distilled water. The solid is then dried overnight in an oven at 110 ° C. and then calcined under a flow of dry air in a crossed bed (1 normal liter per hour and per gram of solid) under the following conditions:
- rise in ambient temperature to 150 ° C at 5 ° C / min,
- one hour stop at 150 ° C,
- rise from 150 to 250 ° C at 5 ° C / min,
- one hour stop at 250 ° C,
- rise from 250 to 350 ° C at 5 ° C / min,
- one hour level at 350 ° C,
- rise from 350 to 520 ° C at 5 ° C / min,
- two hour stop at 520 ° C,
- ambient descent.
Characterizations by X-ray fluorescence, Castaing microprobe and H 2 / O 2 titration provide access to the following results for the solid:
- percentage of platinum (dry mass): 1.7%,
- dispersion of platinum: 82%,
- platinum distribution coefficient: 0.99.
Catalyst A is then prepared by combining the zeolite IZM-2A and the alumina impregnated with platinum as follows. First of all, the granulometry of the starting powders is controlled by sieving ΙΊΖΜ-2 Α and grinding-sieving alumina beads impregnated with platinum to obtain a particle size advantageously less than 63 microns for the two solids. . After weighing the desired solid masses, the mechanical mixing (2 grams dry mass) of the two powders is carried out using a cup mill for 2 minutes, with a ball and a frequency of 30 Hz. The mixture is then pelletized at 4 ton-metric with a Carver hydraulic press, then ground and sieved to the preferred particle size of 250-500 microns. The composition of catalyst A is as follows:
- 10% by weight of the IZM-2 A zeolite,
- 1.5% by weight of platinum,
- 88.5% by weight of impregnated alumina.
Example 2 (according to the invention): preparation of the isomerization catalyst B
Catalyst B is a catalyst comprising an IZM-2 zeolite, platinum, and an alumina matrix. This zeolite IZM-2 was synthesized in accordance with the teaching of the patent FR 2 918 050 B. A colloidal suspension of silica known under the commercial term Ludox HS-40 marketed by Aldrich, is incorporated into a solution composed of soda (Prolabo) , structuring dibromide of 1,6bis (methylpiperidinium) hexane, aluminum hydroxide (Aldrich) and deionized water. The molar composition of the mixture is as follows: 1 SiO 2 , 0.0045 AI 2 O 3 ; 0.1666 Na 2 O; 0.1666 1.6bis (methylpiperidinium) hexane;
33.3333 H 2 O. The mixture is stirred vigorously for half an hour. The mixture is then transferred, after homogenization, to a PARR type autoclave. The autoclave is heated for 5 days at 170 ° C. with stirring in a spit (30 rpm). The product obtained is filtered, washed with deionized water to reach a neutral pH and then dried overnight at 100 ° C in an oven. The solid is then introcLiit in a muffle furnace to be calcined therein in order to remove the structuring agent. The calcination cycle includes a temperature rise up to 200 ° C, a plateau at this temperature of two hours, a temperature rise up to 550 ° C followed by an eight hour plateau at this temperature and finally a return at room temperature. The temperature rises are carried out with a ramp of 2 ° C / min. The solid thus obtained is then refluxed for 2 hours in an aqueous solution of ammonium nitrate (10 ml of solution per gram of solid, concentration of ammonium nitrate of 3 M) in order to exchange the sodium alkaline cations by ammonium ions. This refluxing step is carried out four times with a fresh solution of ammonium nitrate, then the solid is filtered, washed with deionized water and dried in an oven overnight at 100 ° C. Finally, to obtain the zeolite in its acid form (protonated H + ), a calcination step is carried out at 550 ° C for ten hours (temperature rise ramp of 2 ° C / min) in a bed crossed under dry air (2 normal liters per hour and per gram of solid). The solid thus obtained was analyzed by X-ray diffraction and identified as being constituted by the zeolite IZM-2. The zeolite, named IZM-2 B, is used for the preparation of the catalyst. Characterizations using 27 AI NMR, X-ray fluorescence and ICP methods give access to the following results for ΙΊΖΜ2 B:
- weight percentage of hexacoordinated aluminum atoms AIVI: 13%,
- ratio of the number of moles of silicon divided by the number of moles of lattice aluminum, in mole / mole, Si / AI: 91,
- Ratio of the number of moles of sodium divided by the number of moles of lattice aluminum, in mole / mole, Na / Al: 0.28.
For the preparation of catalyst B, the alumina sample impregnated with platinum is used, the preparation of which is described in example 1. Catalyst B is prepared by following the same preparation protocol as for catalyst A of example 1 The composition of catalyst B is as follows:
- 10% by weight of the IZM-2B zeolite,
- 1.5% by weight of platinum,
- 88.5% by weight of impregnated alumina.
Example 3 (according to the invention): preparation of the isomerization catalyst C
Catalyst C is a catalyst comprising an IZM-2 zeolite, platinum, and an alumina matrix. This zeolite IZM-2 was synthesized in accordance with the teaching of patent FR 2 918 050 B. A colloidal suspension of silica known under the commercial name Ludox HS-40 marketed by Aldrich, is incorporated into a solution composed of sodium hydroxide (Prolabo) , structuring dibromide of 1,6bis (methylpiperidinium) hexane, aluminum hydroxide (Aldrich) and deionized water. The molar composition of the mixture is as follows: 1 SiO 2 ; 0.0055 AI 2 O 3 ; 0.1666 Na 2 O; 0.1666 1.6bis (methylpiperidinium) hexane;
33.3333 H 2 O. The mixture is stirred vigorously for half an hour. The mixture is then transferred, after homogenization, to a PARR type autoclave. The autoclave is heated for 5 days at 170 ° C. with stirring in a spit (30 rpm). The product obtained is filtered, washed with deionized water to reach a neutral pH and then dried overnight at 100 ° C in an oven. The solid is then introduced into a muffle furnace to be calcined therein in order to remove the structuring agent. The calcination cycle includes a temperature rise up to 200 ° C, a plateau at this temperature of two hours, a temperature rise up to 550 ° C followed by an eight hour plateau at this temperature and finally a return at room temperature. The temperature rises are carried out with a ramp of 2 ° C / min. The solid thus obtained is then refluxed for 2 hours in an aqueous solution of ammonium nitrate (10 ml of solution per gram of solid, concentration of ammonium nitrate of 3 M) in order to exchange the sodium alkaline cations by ammonium ions. This refluxing step is carried out four times with a fresh solution of ammonium nitrate, then the solid is filtered, washed with deionized water and dried in an oven overnight at 100 ° C. Finally, to obtain the zeolite in its acid form (protonated H + ) a calcination step is carried out at 550 ° C for ten hours (temperature rise ramp of 2 ° C / min) in a bed crossed with dry air (2 normal liters per hour and per gram of solid). The solid thus obtained was analyzed by X-ray diffraction and identified as being constituted by the zeolite IZM-2. The zeolite, named IZM-2 C, is used for the preparation of the catalyst. Characterizations using 27 AI NMR, X-ray fluorescence and ICP methods give access to the following results for ΙΊΖΜ2 C:
- percentage by weight of hexacoordinated aluminum atoms AIVI: 11%,
- ratio of the number of moles of silicon divided by the number of moles of lattice aluminum, in mole / mole, Si / AI: 78,
- Ratio of the number of moles of sodium divided by the number of moles of lattice aluminum, in mole / mole, Na / Al: 0.18.
For the preparation of catalyst C, the alumina sample impregnated with platinum is used, the preparation of which is described in example 1. Catalyst C is prepared by following the same preparation protocol as for catalyst A of example 1. The composition of catalyst C is as follows:
- 10% by weight of the IZM-2 C zeolite,
- 1.5% by weight of platinum,
- 88.5% by weight of impregnated alumina.
Example 4 (according to the invention): preparation of the isomerization catalyst D
Catalyst D is a catalyst comprising an IZM-2 zeolite, platinum, and an alumina matrix. This zeolite IZM-2 was synthesized in accordance with the teaching of patent FR 2 918 050 B. A colloidal suspension of silica known under the commercial name Ludox HS-40 marketed by Aldrich, is incorporated into a solution composed of sodium hydroxide (Prolabo) , structuring dibromide of 1,6bis (methylpiperidinium) hexane, aluminum hydroxide (Aldrich) and deionized water. The molar composition of the mixture is as follows: 1 SiO 2 ; 0.0072 AI 2 O 3 ; 0.1666 Na 2 O; 0.1666 1.6bis (methylpiperidinium) hexane;
33.3333 H 2 O. The mixture is stirred vigorously for half an hour. The mixture is then transferred, after homogenization, to a PARR type autoclave. The autoclave is heated for 5 days at 170 ° C. with stirring in a spit (30 rpm). The product obtained is filtered, washed with deionized water to reach a neutral pH and then dried overnight at 100 ° C in an oven. The solid is then introcLiit in a muffle furnace to be calcined therein in order to remove the structuring agent. The calcination cycle includes a temperature rise up to 200 ° C, a plateau at this temperature of two hours, a temperature rise up to 550 ° C followed by an eight hour plateau at this temperature and finally a return at room temperature. The temperature rises are carried out with a ramp of 2 ° C / min. The solid thus obtained is then refluxed for 2 hours in an aqueous solution of ammonium nitrate (10 ml of solution per gram of solid, concentration of ammonium nitrate of 3 M) in order to exchange the sodium alkaline cations by ammonium ions. This refluxing step is carried out four times with a fresh solution of ammonium nitrate, then the solid is filtered, washed with deionized water and dried in an oven overnight at 100 ° C. Finally, to obtain the zeolite in its acid form (protonated H + ) a calcination step is carried out at 550 ° C for ten hours (temperature rise ramp of 2 ° C / min) in a bed crossed with dry air (2 normal liters per hour and per gram of solid). The solid thus obtained was analyzed by X-ray diffraction and identified as being constituted by the zeolite IZM-2. The zeolite, called IZM-2D, is used for the preparation of the catalyst. Characterizations using 27 AI NMR, X fluorescence and ICP methods give access to the following results for ΙΊΖΜ2 D:
- percentage by weight of hexacoordinated aluminum atoms AIVI: 12%,
- ratio of the number of moles of silicon divided by the number of moles of lattice aluminum, in mole / mole, Si / AI: 63,
- Ratio of the number of moles of sodium divided by the number of moles of lattice aluminum, in mole / mole, Na / Al: 0.19.
For the preparation of catalyst D, the alumina sample impregnated with platinum is used, the preparation of which is described in Example 1. Catalyst D is prepared by following the same preparation protocol as for catalyst A of Example 1 The composition of catalyst D is as follows:
- 10% by weight of the IZM-2 D zeolite,
- 1.5% by weight of platinum,
- 88.5% by weight of impregnated alumina.
Example 5 (not in accordance with the invention): preparation of the isomerization catalyst E
Catalyst E is a catalyst comprising an IZM-2 zeolite, platinum, and an alumina matrix. This zeolite IZM-2 was synthesized in accordance with the teaching of the patent FR 2 918 050 B. A colloidal suspension of silica known under the commercial term Ludox HS-40 marketed by Aldrich, is incorporated into a solution composed of soda (Prolabo) , structuring dibromide of 1,6bis (methylpiperidinium) hexane, aluminum hydroxide (Aldrich) and deionized water. The molar composition of the mixture is as follows: 1 SiO 2 ; 0.0100 AI 2 O 3 ; 0.1666 Na 2 O; 0.1666 1.6bis (methylpiperidinium) hexane;
33.3333 H 2 O. The mixture is stirred vigorously for half an hour. The mixture is then transferred, after homogenization, to a PARR type autoclave. The autoclave is heated for 5 days at 170 ° C. with stirring in a spit (30 rpm). The product obtained is filtered, washed with deionized water to reach a neutral pH and then dried overnight at 100 ° C in an oven. The solid is then introduced into a muffle furnace to be calcined there in order to remove the structuring agent. The calcination cycle includes a temperature rise up to 200 ° C, a plateau at this temperature of two hours, a temperature rise up to 550 ° C followed by an eight hour plateau at this temperature and finally a return at room temperature. The temperature rises are carried out with a ramp of 2 ° C / min. The solid thus obtained is then refluxed for 2 hours in an aqueous solution of ammonium nitrate (10 ml of solution per gram of solid, concentration of ammonium nitrate of 3 M) in order to exchange the sodium alkaline cations by ammonium ions. This refluxing step is carried out four times with a fresh solution of ammonium nitrate, then the solid is filtered, washed with deionized water and dried in an oven overnight at 100 ° C. Finally, to obtain the zeolite in its acid form (protonated H + ) a calcination step is carried out at 550 ° C for ten hours (temperature rise ramp of 2 ° C / min) in a bed crossed with dry air (2 normal liters per hour and per gram of solid). The solid thus obtained was analyzed by X-ray diffraction and identified as being constituted by the zeolite IZM-2. The zeolite, named IZM-2 E, is used for the preparation of the catalyst. Characterizations by 27 AI NMR, X fluorescence and ICP provide access to the following results for ΙΊΖΜ-2 Ε:
- weight percentage of hexacoordinated aluminum atoms AIVI: 6%,
- ratio of the number of moles of silicon divided by the number of moles of lattice aluminum, in mole / mole, Si / AI: 46,
- Ratio of the number of moles of sodium divided by the number of moles of lattice aluminum, in mole / mole, Na / Al: 0.08.
For the preparation of catalyst E, the sample of alumina impregnated with platinum is used, the preparation of which is described in example 1. Catalyst E is prepared by following the same preparation protocol as for catalyst A of example 1 The composition of catalyst E is as follows:
- 10% by weight of the IZM-2E zeolite,
- 1.5% by weight of platinum,
- 88.5% by weight of impregnated alumina.
Example 6: Evaluation of the catalytic properties of catalysts A, B, C, D, E, in isomerization of a C "aromatic cut
The catalysts were tested in isomerization of an aromatic C 8 cut composed of ethylbenzene (19% by weight), ortho-xylene (16% by weight), meta-xylene (58% by weight) and l 'ethylcyclohexane (7% by weight). The tests were carried out in a micro-unit implementing a fixed bed reactor and working in downdraft without recycling. The analysis of the hydrocarbon effluents is carried out online by gas chromatography. Before loading into the unit, the catalyst is dried beforehand for at least one night in an oven at 110 ° C. Once loaded in the unit, the cafelyseur undergoes a first stage of drying under nitrogen under the following conditions:
- nitrogen flow: 5 normal liters per hour and per gram of catalyst,
- total pressure: 1.3 MPa,
- ramp up to ambient temperature at 150 ° C: 10 ° C / min,
- level at 150 ° C for 30 minutes.
After drying, the nitrogen is replaced by hydrogen and a reduction step under flow of pure hydrogen is then carried out under the following conditions:
- hydrogen flow: 4 normal liters per hour and per gram of catalyst,
- total pressure: 1.3 MPa,
- temperature rise ramp from 150 to 480 ° C: 5 ° Cmin,
- stop at 480 ° C for 2 hours.
The temperature then dropped to 425 ° C. and then the catalyst was stabilized for 24 hours under a stream of hydrogen and hydrocarbons (mixture of ethylbenzene at 20% by weight and ortho-xylene at 80% by weight), under the conditions following operations:
- space feeding speed of 5 grams of hydrocarbons per hour and per gram of catalyst,
- molar ratio hydrogen to hydrocarbons of 4,
- total pressure of 1.3 MPa.
After the stabilization step, the temperature then dropped to 385 ° C., and the catalyst is brought into contact with the aromatic C 8 cut mentioned above under the following conditions:
- space feeding speed of 3.5 grams of the C8 aromatic cut per hour and per gram of catalyst,
- molar ratio hydrogen to hydrocarbons of 4,
- total pressure of 0.86 MPa.
The catalyst is maintained for 7 hours under these operating conditions and then the catalytic performance is evaluated according to the various operating conditions which are summarized in Table 2 below. The variation in the space feeding speed makes it possible to vary the levels of conversion to ethylbenzene and of isomerization of the xylenes and therefore the production of para-xylene. At each operating condition, two analyzes by chromatography are carried out in order to measure the performance of the catalysts.
Table 2: operating conditions implemented for the catalytic evaluation
conditions 1 2 3 4 5 6 Duration at each condition (h) 2.8 2.1 2.1 2.1 2.1 2.1 Temperature (° C) 385 385 385 385 385 385 Spatial feeding speed (h 1 ) 3.5 4.5 6.0 9.0 12.0 20.0 H 2 / hydrocarbons (mole / mole) 4 4 4 4 4 4 Total pressure (MPa) 0.86 0.86 0.86 0.86 0.86 0.86
The yield of para-xylene (PX) in the hydrocarbon effluent obtained at the space feed speed of 20 h 1 makes it possible to evaluate the activity of the catalysts for the production of para-xylene:
PX =% by weight of para-xylene in the hydrocarbon effluent, where PX is the yield of para-xylene in% by weight.
The evolution of the yield in net losses (PN) as a function of the para-xylene yield makes it possible to assess the selectivity of the catalyst. All hydrocarbon molecules other than cyclic molecules with eight carbon atoms are considered to be net losses:
PN = 100-PX-EB-OX-MX-N8 with:
PN: yield in net losses in the hydrocarbon effluent, in% by weight,
PX:% by weight of para-xylene in the hydrocarbon effluent,
EB:% by weight of ethylbenzene in the hydrocarbon effluent,
OX:% by weight of ortho-xylene in the hydrocarbon effluent,
MX:% by weight of meta-xylene in the hydrocarbon effluent,
N8:% by weight of naphthenes containing eight carbon atoms in the hydrocarbon effluent.
Table 3 thus reports the para-xylene yield of catalysts A, B, C, D and E at a space speed of 20 h 1 as well as the estimated net losses for a para-xylene yield of 18% for the catalysts. The net losses (PN) at 18% yield in para-xylene are estimated by linear interpolation or extrapolation of experimental data of the evolution of the yield in net losses as a function of the yield in para-xylene. Catalysts A, B, C, D and E are distinguished only by the nature of the IZM-2 zeolite used in their composition.
Catalyst E, which involves ΙΊΖΜ-2 Ε with an Si / Al ratio of 46, is the most active catalyst 5 of all the catalysts, but on the other hand it is much less selective than the other catalysts. Catalyst A, which involves ΙΊΖΜ-2 Α with an Si / Al ratio of 113, is the least active solid of all the catalysts, while its selectivity remains comparable to that of catalysts B, C, D. Ultimately, l '' use of IZM-2 B zeolites (Si / AI of 91),
C (Si / AI of 78) and D (Si / AI of 63) makes it possible to obtain better activity than with zeolite 10 IZM-2 A (Si / AI of 113) and better selectivity than with zeolite IZM-2 E (Si / AI of 46).
Table 3: catalytic performances of catalysts A, B, C, D and E
Catalyst AT B VS D E Si / AI molar ratio (IZM-2) 113 91 78 63 46 Para-xylene yield at 20 h 1 space speed 7.6 12.6 14.7 16.6 17.7 Net loss yield at 18% para-xylene yield 2.5 2.8 2.6 2.8 3.8
权利要求:
Claims (13)
[1" id="c-fr-0001]
1. Catalyst comprising at least one IZM-2 zeolite, at least one matrix and at least one metal from group VIII of the periodic table, said catalyst being characterized in that the ratio between the number of moles of silicon and the number of aluminum moles of the IZM-2 zeolite is between 60 and 150.
[2" id="c-fr-0002]
2. Catalyst according to claim 1 in which the ratio between the number of moles of silicon and the number of moles of aluminum of the zeolite IZM-2 is between 60 and 110.
[3" id="c-fr-0003]
3. Catalyst according to claim 1 or 2 in which the ratio between the number of moles of silicon and the number of moles of aluminum of the IZM-2 zeolite is between 60 and 95.
[4" id="c-fr-0004]
4. Catalyst according to one of the preceding claims, in which the zeolite IZM-2 present is in its acid form.
[5" id="c-fr-0005]
5. Catalyst according to one of the preceding claims, in which said matrix is chosen from the group formed by alumina, silica, silica-alumina, clays, titanium oxide, boron oxide and zirconia , taken alone or as a mixture, or aluminates.
[6" id="c-fr-0006]
6. Catalyst according to claim 5 in which the matrix is alumina.
[7" id="c-fr-0007]
7. Catalyst according to one of the preceding claims in which the group VIII metal is chosen from iron, cobalt, nickel, ruthenium, rhodium, palladium, osmium, iridium and platinum, preferably from the noble metals of group VIII, very preferably from palladium and platinum, and even more preferably platinum.
[8" id="c-fr-0008]
8. Catalyst according to one of the preceding claims comprising at least one additional metal chosen from the group formed by the metals of groups IIIA, IVA and VIIB of the periodic table of the elements and preferably from gallium, indium, tin and rhenium.
[9" id="c-fr-0009]
9. Catalyst according to one of the preceding claims further comprising sulfur.
[10" id="c-fr-0010]
10. Catalyst according to one of the preceding claims comprising:
- from 1 to 90% of the IZM-2 zeolite,
- from 0.01 to 4% of at least one metal from group VIII of the periodic table,
5 - optionally from 0.01 to 2% of at least one additional metal chosen from the group formed by the metals of groups IIIA, IVA and VIIB,
- optionally a sulfur content such that the ratio of the number of moles of sulfur to the number of moles of group VIII metal (s) is between 0.3 and 3,
10 - at least one matrix ensuring the complement to 100% in the catalyst.
[11" id="c-fr-0011]
11. A process for isomerizing a cut containing at least one aromatic compound containing eight carbon atoms per molecule, said process comprising bringing said aromatic cut into contact with at least the catalyst according to one of the preceding claims under the conditions following operations:
[12" id="c-fr-0012]
15 - a temperature of 300 ° C to 500 ° C,
- a partial hydrogen pressure of 0.3 to 1.5 MPa,
- a total pressure of 0.45 to 1.9 MPa, and
- a spatial feed speed, expressed in kilograms of feed introduced per kilogram of catalyst and per hour, from 0.25 to 30 h 1 .
[13" id="c-fr-0013]
12. The isomerization process according to claim 11 wherein said aromatic cut containing at least one aromatic compound having eight carbon atoms per molecule comprises as aromatic compound having eight carbon atoms per molecule either only a mixture of xylenes or only of ethylbenzene, a mixture of xylene (s) and ethylbenzene.
类似技术:
公开号 | 公开日 | 专利标题
EP3275538B1|2020-06-24|Process for the isomerisation of aromatic c8 fractions with a catalyst comprising zeolite izm-2 having a molar si/al ratio optimised for the isomerisation of aromatic c8 fractions
EP2313343B1|2012-11-14|Catalyst comprising an izm-2 zeolite and at least one metal and use thereof in the conversion of hydrocarbons
EP0946416B1|2002-02-20|Im-5 zeolite, method of preparation and catalytic applications thereof
EP0825152B1|2002-01-23|Zeolite NU-88, method for its preparation and its catalytic uses
EP1985600B1|2020-05-06|Method for isomerising an aromatic C8 fraction in the presence of a catalyst made from a dealuminated EUO zeolite
EP1932819B1|2009-09-30|Isomerisation method for aromatic C8 compounds in the presence of a catalyst including a modified EUO zeolite
EP0755717B1|2000-05-24|Mordenite zeolite catalysts modified with cerium and use thereof for the isomerisation of an aromatic C8 fraction
EP3027312B1|2020-01-08|Modification of euo type zeolite and use thereof in isomerization of aromatic c8 compounds
EP1151963B1|2011-06-22|EUO-type zeolite with reduced SI/AL ratio and its use as a catalyst for the isomerization of C8 fractions
CA2346312C|2010-09-28|Process for producing a zeolite with a euo structure, the zeolite thus produced and its use as a catalyst for the isomerization of c8 aromatic fractions
WO2018099832A1|2018-06-07|Use of a catalyst based on izm-2 zeolite and a catalyst based on euo zeolite for the isomerisation of aromatic c8 fractions
WO2021122199A1|2021-06-24|Izm-2 zeolite catalyst having a low alkali content, and use thereof for the isomerization of the aromatic c8 fraction
EP3581634B1|2021-01-20|Use of a bifunctional catalyst made of izm-2 with specific si/al ratio for the isomerisation of long paraffin charges into medium distillates
EP1985363B1|2010-09-01|Modified EU-1 zeolite and its use for isomerising aromatic C8 compounds
WO2014096606A1|2014-06-26|Modified catalyst having an mtw structure, method for preparing same and use thereof in a method for isomerising an aromatic c8 cut
FR3074428A1|2019-06-07|PROCESS FOR THE PREPARATION OF A IZM-2 CATALYST FROM A SOLUTION COMPRISING SPECIFIC PRECURSORS AND USE FOR THE ISOMERIZATION OF PARAFFINIC CHARGES
FR2997948A1|2014-05-16|PROCESS FOR ISOMERIZING AN AROMATIC C8 CUT IN THE PRESENCE OF A CATALYST BASED ON A EUO ZEOLITE AND A PARTICULAR SODIUM CONTENT
WO2021122198A1|2021-06-24|Use of a catalyst based on izm-2 with a low content of alkali metal for the isomerization of paraffinic feedstocks to middle distillates
WO2013093222A1|2013-06-27|Method for isomerizing an aromatic c8 fraction in the presence of a catalyst containing an euo zeolite and a specific binder
FR2901716A1|2007-12-07|USE OF ITQ-6 ZEOLITE CATALYST IN ISOMERIZATION OF C8 AROMATIC CUTTING
同族专利:
公开号 | 公开日
US20180029957A1|2018-02-01|
EP3275538A1|2018-01-31|
US10183902B2|2019-01-22|
JP2018030833A|2018-03-01|
CN107774301A|2018-03-09|
DK3275538T3|2020-09-21|
EP3275538B1|2020-06-24|
JP6955925B2|2021-10-27|
FR3054454B1|2020-04-10|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
WO2010015733A1|2008-08-08|2010-02-11|Ifp|Catalyst comprising an izm-2 zeolite and at least one metal and use thereof in the conversion of hydrocarbons|
WO2013153317A1|2012-04-11|2013-10-17|IFP Energies Nouvelles|Method for the dewaxing of hydrocarbon feedstocks using an izm-2 zeolite-based catalyst|EP3581634A1|2018-06-15|2019-12-18|IFP Energies nouvelles|Use of a bifunctional catalyst made of izm-2 with specific si/al ratio for the isomerisation of long paraffin charges into medium distillates|
FR3104458A1|2019-12-17|2021-06-18|IFP Energies Nouvelles|ZEOLITHE IZM-2 BASED CATALYST WITH LOW ALKALINE CONTENT AND ITS USE FOR ISOMERIZATION OF C8 AROMATIC CUP|FR2477903B1|1980-03-13|1984-06-15|Inst Francais Du Petrole|
US4482773A|1982-02-25|1984-11-13|Mobil Oil Corporation|Catalyst for xylene isomerization|
US4467129A|1982-11-24|1984-08-21|Toray Industries, Inc.|Conversion of xylenes containing ethylbenzene|
FR2642414B1|1989-02-01|1991-04-26|Rhone Poulenc Chimie|PROCESS FOR THE MANUFACTURE OF AGGLOMERATES OF ACTIVE ALUMIN, AGGLOMERATES OBTAINED BY THE PROCESS AND DEVICE FOR IMPLEMENTING SAME|
US6440980B1|1996-09-17|2002-08-27|Avanir Pharmaceuticals|Synergistic inhibition of viral replication by long-chain hydrocarbons and nucleoside analogs|
EP0923987A1|1997-12-22|1999-06-23|Institut Français du Pétrole|Catalyst comprising a zeolithe EUO and its use in the isomerisation of aromatic C8 compounds|
CN100512954C|2003-12-30|2009-07-15|环球油品公司|Process and bimetallic catalyst for c alkyl aromatic isomerization|
FR2918050B1|2007-06-29|2011-05-06|Inst Francais Du Petrole|IZM-2 CRYSTALLIZED SOLID AND PROCESS FOR PREPARING THE SAME|
BRPI0914603A2|2008-07-04|2015-12-08|Shell Internationale Res Maartschappij B V|alkylaromatic isomerization catalyst; and, process for the isomerization of alkylaromatics to provide a reaction mixture.|
FR2969511B1|2010-12-22|2012-12-28|IFP Energies Nouvelles|SPHERICAL MATERIAL COMPRISING METALLIC NANOPARTICLES TRAPPED IN A MESOSTRUCTURED OXIDE MATRIX AND ITS USE AS CATALYST IN REFINING PROCESSES|
US20140296601A1|2013-03-29|2014-10-02|Uop Llc|Isomerization process with mtw catalyst|FR3074428B1|2017-12-06|2022-01-21|Ifp Energies Now|METHOD FOR THE PREPARATION OF A CATALYST BASED ON IZM-2 FROM A SOLUTION COMPRISING SPECIFIC PRECURSORS AND USE FOR THE ISOMERIZATION OF PARAFFINIC CHARGERS|
CN108993585B|2018-08-20|2021-04-02|中触媒新材料股份有限公司|Bifunctional catalyst containing hierarchical pore EUO molecular sieve and preparation method thereof|
法律状态:
2017-07-31| PLFP| Fee payment|Year of fee payment: 2 |
2018-02-02| PLSC| Publication of the preliminary search report|Effective date: 20180202 |
2018-07-25| PLFP| Fee payment|Year of fee payment: 3 |
2019-07-25| PLFP| Fee payment|Year of fee payment: 4 |
2020-07-28| PLFP| Fee payment|Year of fee payment: 5 |
2021-07-26| PLFP| Fee payment|Year of fee payment: 6 |
优先权:
申请号 | 申请日 | 专利标题
FR1657146|2016-07-26|
FR1657146A|FR3054454B1|2016-07-26|2016-07-26|CATALYST COMPRISING AN IZM-2 ZEOLITE HAVING AN OPTIMIZED IF / AL MOLAR RATIO FOR THE ISOMERIZATION OF C8 AROMATIC CUTS|FR1657146A| FR3054454B1|2016-07-26|2016-07-26|CATALYST COMPRISING AN IZM-2 ZEOLITE HAVING AN OPTIMIZED IF / AL MOLAR RATIO FOR THE ISOMERIZATION OF C8 AROMATIC CUTS|
JP2017142366A| JP6955925B2|2016-07-26|2017-07-24|Catalyst containing IZM-2 zeolite with optimized Si / Al molar ratio for isomerization of C8 aromatic fractions|
EP17305989.0A| EP3275538B1|2016-07-26|2017-07-25|Process for the isomerisation of aromatic c8 fractions with a catalyst comprising zeolite izm-2 having a molar si/al ratio optimised for the isomerisation of aromatic c8 fractions|
US15/658,900| US10183902B2|2016-07-26|2017-07-25|Catalyst comprising an IZM-2 zeolite with an optimized Si/Al molar ratio, for the isomerization of C8 aromatic cuts|
DK17305989.0T| DK3275538T3|2016-07-26|2017-07-25|PROCEDURE FOR ISOMERIZATION OF AROMATIC C8 FRACTIONS WITH A CATALYZER INCLUDING A ZEOLITE IZM-2, WITH A MOLE RATIO SI / AL, OPTIMIZED FOR ISOMERIZATION OF AROMATIC C8-FRA|
CN201710617072.4A| CN107774301A|2016-07-26|2017-07-26|The catalyst for including the zeolites of IZM 2 with optimization Si/Al mol ratios for the isomerization of C8 aromatic fractions|