专利摘要:
The invention relates to a rubber composition having an improved processability / stiffness compromise, said composition being based on at least one diene elastomer, a reinforcing filler, a crosslinking system, between 1 and 30 parts by weight per hundred parts by weight. elastomer weight, phr, of an epoxy resin and between 1 and 15 phr of a specific amine hardener comprising in particular at least two primary amine functions located on at least one aromatic ring with six atoms and at least two identical radicals R 1, or different, selected from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and ethers, tertiary amines, thioethers, ketones, esters and amides, substituted by alkyl radicals linear or branched C1-C6, said ring not comprising a hydrogen atom located ortho position with respect to the primary amine functions.
公开号:FR3053344A1
申请号:FR1656142
申请日:2016-06-30
公开日:2018-01-05
发明作者:Emmanuel Landreau;Philippe Laubry
申请人:Michelin Recherche et Technique SA Switzerland ;Compagnie Generale des Etablissements Michelin SCA;Michelin Recherche et Technique SA France;
IPC主号:
专利说明:

Holder (s): COMPAGNIE GENERALE DES ETABLISSEMENTS MICHELIN Limited partnership with shares, MICHELIN RECHERCHE ET TECHNIQUE S.A. Limited company.
Extension request (s)
Agent (s): MANUF FSE PNEUMATIQUES MICHELIN Limited partnership with shares.
RUBBER COMPOSITION COMPRISING AN EPOXIDE RESIN AND A SPECIFIC AMINE HARDENER.
FR 3 053 344 - A1
The invention relates to a rubber composition having an improved processability / rigidity compromise, said composition being based on at least one diene elastomer, a reinforcing filler, a crosslinking system, between 1 and 30 parts by weight per hundred parts weight of elastomer, phr, of an epoxy resin and between 1 and 15 phr of a specific amine hardener comprising in particular at least two primary amine functions located on at least one aromatic ring with six atoms and at least two identical radicals Ri or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and ethers, tertiary amines, thioethers, ketones, esters and amides, substituted by alkyl radicals linear or branched in C1C6, said cycle not comprising a hydrogen atom located in the ortho position with respect to the primary amine functions.
-1 RUBBER COMPOSITION COMPRISING AN EPOXIDE RESIN AND A SPECIFIC AMINE HARDENER
The present invention relates to rubber compositions intended in particular for the manufacture of tires or semi-finished products for tires, in particular rubber compositions having a high rigidity.
It is known to use in certain parts of tires, rubber compositions having a high rigidity during slight deformations of the tire as presented in application WO 02/10269. Resistance to low deformation is one of the properties that a tire must have in order to respond to the stresses to which it is subjected.
This stiffening can be obtained by increasing the rate of reinforcing filler or by incorporating certain reinforcing resins in the rubber compositions constituting the parts of the tire.
The reinforcing resins conventionally used to increase the rigidity of the compositions are reinforcing resins based on an acceptor / donor methylene system. The terms “methylene acceptor” and “methylene donor” are well known to those skilled in the art and widely used to denote compounds capable of reacting together to generate by condensation a three-dimensional reinforcing resin which comes to superimpose, interpenetrate with the reinforcing filler / elastomer network on the one hand, with the elastomer / sulfur network on the other hand (if the crosslinking agent is sulfur). With the methylene acceptor described above is associated a hardening agent, capable of crosslinking or hardening, also commonly called "methylene donor". The crosslinking of the resin is then caused during the curing of the rubber matrix, by formation of methylene bridges between the carbons in ortho and para positions of the phenolic nuclei of the resin and the methylene donor, thus creating a three-dimensional resin network. .
Conventionally, the methylene acceptor is a phenolic resin. Novolak phenolic resins have already been described in rubber compositions,
-2 in particular intended for tires or tire treads, for applications as varied as adhesion or reinforcement: reference will be made for example to patent EP 0 649 446. Furthermore, the methylene donors conventionally used are hexa-methylenetetramine (abbreviated HMT), or hexamethoxymethylmelamine (abbreviated HMMM or H3M), or hexaethoxymethylmelamine.
However, the combination of a phenolic resin, methylene acceptor with HMT or 1Μ3Μ methylene donor, produces formaldehyde during the vulcanization of the rubber composition. However, it is desirable to reduce or even eliminate formaldehyde from rubber compositions in the long term because of the potential environmental impact of these compounds.
To this end, alternative compositions to the compositions comprising the methylene-acceptor formo-phenolic resin pair with a conventional HMT or H3M hardener methylene donor have been developed. By way of example, application WO 2011/045342 describes compositions comprising an epoxy resin couple with an amine hardener. These compositions, in addition to the advantage of eliminating the formation of formaldehyde, exhibit, after crosslinking, stiffnesses greater than conventional compositions while retaining an acceptable rolling resistance. However, it is always desirable to improve the raw properties of these compositions, in particular their processability, so as to facilitate the production of these compositions and thus reduce the overall production costs, while maintaining a good level of rigidity.
Statement of the invention
Unexpectedly, the Applicants discovered during their research that the choice of a particular amine hardener with an epoxy resin makes it possible to improve the processability of the rubber compositions before curing (raw), in particular the roasting time or the viscosity of these compositions, compared to the compositions used to date. Thus, the compositions in accordance with the present invention exhibit a processability / rigidity compromise much higher than that of known compositions.
- 3 Consequently, a first subject of the invention relates to a rubber composition based on at least:
- a diene elastomer;
- a reinforcing filler;
- a crosslinking system;
- between 1 and 30 parts by weight per hundred parts by weight of elastomer, pce, of an epoxy resin;
- between 1 and 15 phr of an amino hardener comprising at least two primary amine functions located on at least one six-atom aromatic ring, said at least one six-atom aromatic ring comprising:
o at least one primary amine function, and o at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens and ethers, tertiary amines, thio -ethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals, so that the at least one six-atom aromatic ring does not contain a hydrogen atom located in position ortho to the primary amine functions, said amino hardener comprising at least one second primary amine function located on said at least one six-atom aromatic ring or on a possible second six-atom aromatic ring of said amino hardener.
A subject of the invention is also finished or semi-finished rubber articles for tires and tires comprising a rubber composition in accordance with the invention, as well as a process for preparing the composition according to the invention.
The invention as well as its advantages will be easily understood in the light of the description and of the exemplary embodiments which follow.
-4Definitions
By the expression part by weight per hundred parts by weight of elastomer (or phr), it is understood within the meaning of the present invention, the part, by mass per hundred parts by mass of elastomer or rubber.
In the present document, unless expressly indicated otherwise, all the percentages (%) indicated are percentages (%) by mass.
On the other hand, any range of values designated by the expression between a and b represents the range of values going from more than a to less than b (i.e. limits a and b excluded) while any range of values designated by the expression from a to b signifies the range of values going from a to b (that is to say including the strict limits a and b). In the present, when we designate a range of values by the expression from a to b, we also and preferably designate the range represented by the expression between a and b.
In the present, by the expression composition based on, is meant a composition comprising the mixture and / or the reaction product of the various constituents used, some of these base constituents being capable of, or intended to react with each other, at least in part, during the various manufacturing phases of the composition, in particular during its crosslinking or vulcanization. By way of example, a composition based on an elastomeric matrix and on sulfur comprises the elastomeric matrix and the sulfur before cooking, whereas after cooking the sulfur is no longer detectable because the latter reacted with the elastomeric matrix. forming sulfur bridges (polysulfides, disulfides, mono-sulfide).
When reference is made to a “majority” compound, it is understood within the meaning of the present invention, that this compound is predominant among the compounds of the same type in the composition, that is to say that it is that which represents the greatest amount by mass among the compounds of the same type, for example more than 50%, 60%, 70%, 80%, 90%, or even 100% by weight relative to the total weight of the type of compound. Thus, for example, a majority reinforcing filler is the reinforcing filler representing the largest mass relative to the total mass of the reinforcing fillers in the composition. At
On the contrary, a “minority” compound is a compound which does not represent the largest mass fraction among the compounds of the same type.
In the context of the invention, the carbon products mentioned in the description can be of fossil origin or bio-based. In the latter case, they can be, partially or totally, from biomass or obtained from renewable raw materials from biomass. Are concerned in particular polymers, plasticizers, fillers, etc.
Elastomeric matrix
The composition of the tire of the invention may contain a single diene elastomer or a mixture of several diene elastomers.
By elastomer (or “rubber”, the two terms being considered as synonyms) of the diene type, it is recalled here that must be understood in known manner one (means one or more) elastomer derived at least in part (ie, a homopolymer or a copolymer) of diene monomers (monomers carrying two carbon-carbon double bonds, conjugated or not).
These diene elastomers can be classified into two categories: essentially unsaturated or essentially saturated. Generally understood by essentially unsaturated, a diene elastomer derived at least in part from conjugated diene monomers, having a rate of units or units of diene origin (conjugated dienes) which is greater than 15% (% by moles); This is how diene elastomers such as butyl rubbers or copolymers of dienes and of alpha-olefins of the EPDM type do not enter into the preceding definition and can be qualified in particular as essentially saturated diene elastomers (rate of units d weak or very weak diene origin, always less than 15%). In the category of essentially unsaturated diene elastomers, the term “highly unsaturated diene elastomer” is understood to mean in particular a diene elastomer having a content of units of diene origin (conjugated dienes) which is greater than 50%.
These definitions being given, the term “diene elastomer capable of being used in the compositions in accordance with the invention” is understood more particularly to be:
(a) any homopolymer obtained by polymerization of a conjugated diene monomer having from 4 to 12 carbon atoms;
(b) any copolymer obtained by copolymerization of one or more dienes conjugated together or with one or more vinyl aromatic compounds having from 8 to 20 carbon atoms;
(c) a ternary copolymer obtained by copolymerization of ethylene, of an α-olefin having 3 to 6 carbon atoms with a non-conjugated diene monomer having of 6 to 12 carbon atoms, such as for example the elastomers obtained from ethylene, propylene with a non-conjugated diene monomer of the aforementioned type such as in particular 1,4-hexadiene, ethylidene norbornene, dicyclopentadiene;
(d) a copolymer of isobutene and isoprene (butyl rubber), as well as the halogenated, in particular chlorinated or brominated, versions of this type of copolymer.
Although it applies to any type of diene elastomer, a person skilled in the art of tires will understand that the present invention is preferably implemented with essentially unsaturated diene elastomers, in particular of the type (a) or (b ) above.
As conjugated dienes, 1,3-butadiene, 2-methyl-1,3butadiene, 2,3-di (C1-C5 alkyl) -1,3-butadienes such as, for example, 2,3-dimethyl are suitable. -1.3-butadiene, 2,3-diethyl-1,3-butadiene, 2-methyl-3-ethyl-1,3-butadiene, 2-methyl-3-isopropyl-1,3-butadiene, aryl-1,3-butadiene, 1,3-pentadiene, 2,4hexadiene. Examples of vinyl aromatic compounds are styrene, ortho-, meta-, para-methylstyrene, the commercial vinyl-toluene mixture, paratertiobutylstyrene, methoxystyrenes, chlorostyrenes, vinylmesitylene, divinylbenzene, vinylnaphthalene.
The copolymers can contain between 99% and 20% by weight of diene units and between 1% and 80% by weight of vinyl aromatic units. Elastomers can have any
-7microstructure which is a function of the polymerization conditions used, in particular the presence or absence of a modifying and / or randomizing agent and the quantities of modifying and / or randomizing agent used. The elastomers can be, for example, block, statistical, sequenced, microsequenced, and be prepared in dispersion or in solution; they can be coupled and / or starred or functionalized with a coupling and / or star-forming or functionalizing agent. For coupling to carbon black, mention may, for example, be made of functional groups comprising a C-Sn bond or amine functional groups such as aminobenzophenone for example; for coupling to a reinforcing inorganic filler such as silica, mention may, for example, be made of silanol or polysiloxane functional groups having a silanol end (as described for example in FR 2 740 778 or US 6 013 718 and WO 2008/141702), alkoxysilane groups (as described for example in FR 2 765 882 or US 5 977 238), carboxylic groups (as described for example in WO 01/92402 or US 6 815 473, WO 2004/096865 or US 2006/0089445 ) or also polyether groups (as described for example in EP 1 127 909 or US 6 503 973, WO 2009/000750 and WO 2009/000752). As other examples of functionalized elastomers, mention may also be made of elastomers (such as SBR, BR, NR or IR) of the epoxidized type.
In summary, the diene elastomer of the composition can be chosen, for example, from the group of highly unsaturated diene elastomers constituted by natural rubber (NR), synthetic polyisoprenes (IR), polybutadienes (abbreviated as BR), butadiene copolymers, isoprene copolymers and mixtures of these elastomers. Such copolymers are more preferably chosen from the group consisting of butadiene-styrene copolymers (SBR), isoprene butadiene copolymers (BIR), isoprene-styrene copolymers (SIR), isoprene butadiene-styrene copolymers ( SBIR), butadiene-acrylonitrile copolymers (NBR), butadiene-styrene-acrylonitrile copolymers (NSBR) or a mixture of two or more of these compounds.
According to a particular preferred embodiment, the diene elastomer is a predominantly isoprene elastomer. The term isoprene elastomer is understood to mean, in known manner, an isoprene homopolymer or copolymer, in other words a
- 8 diene elastomer chosen from the group consisting of natural rubber (NR) which can be plasticized or peptized, synthetic polyisoprenes (IR), the various isoprene copolymers and mixtures of these elastomers. Among the isoprene copolymers, mention will be made in particular of isobutene-isoprene (butyl rubber IIR), isoprene-styrene (SIR), isoprene-butadiene (BIR) or isoprene butadiene-styrene (SBIR) copolymers .
The diene elastomer is preferably chosen from the group consisting of natural rubber, synthetic polyisoprenes and their mixtures. Among these synthetic polyisoprenes, polyisoprenes are preferably used having a rate (mol%) of cis 1,4 bonds greater than 90%, more preferably still greater than 98%. More preferably, the diene elastomer is natural rubber.
Preferably, the level of diene elastomer, preferably isoprene elastomer, preferably natural rubber, is from 50 to 100 phr, more preferably from 60 to 100 phr, more preferably from 70 to 100 phr, even more preferably from 80 to 100 pce and very preferably 90 to 100 pce. In particular, the level of diene elastomer, preferably isoprene elastomer, more preferably natural rubber, is very preferably 100 phr.
Whether they contain a single diene elastomer or a mixture of several diene elastomers, the compositions of the invention can be used in combination with any type of synthetic elastomer other than diene, or even with polymers other than elastomers, for example thermoplastic polymers.
Reinforcing filler
The composition of the tire according to the invention advantageously comprises a reinforcing filler, known for its capacity to reinforce a rubber composition which can be used for the manufacture of tires.
The reinforcing filler can comprise carbon black, an organic filler other than carbon black, an inorganic filler or the mixture of at least two of these
-9 loads. Preferably, the reinforcing filler can comprise carbon black, an inorganic reinforcing filler, preferably silica, or a mixture of carbon black and inorganic reinforcing filler, preferably silica. More preferably still, the reinforcing filler mainly, or even exclusively, comprises carbon black, in particular in the case where the composition is used in an internal layer. The reinforcing filler may also mainly comprise an inorganic reinforcing filler, in particular in the case where the composition is used in a tread.
Such a reinforcing filler typically consists of particles whose average size (by mass) is less than a micrometer, generally less than 500 nm, most often between 20 and 200 nm, in particular and more preferably between 20 and 150 nm.
The blacks which can be used in the context of the present invention may be any black conventionally used in tires or their treads (so-called pneumatic grade blacks). Among the latter, there may be mentioned more particularly the reinforcing carbon blacks of the 100, 200, 300 series, or the blacks of the 500, 600 or 700 series (ASTM grades), such as, for example, the blacks NI 15, N134, N234, N326, N330, N339, N347, N375, N550, N683, N772). These carbon blacks can be used in the isolated state, as commercially available, or in any other form, for example as a support for some of the rubber additives used. The carbon blacks could, for example, already be incorporated into the diene elastomer, in particular isoprene, in the form of a masterbatch (see for example applications WO 97/36724 or WO 99/16600). The BET specific surface area of carbon blacks is measured according to standard D6556-10 [multipoint method (at least 5 points) - gas: nitrogen - relative pressure range Ρ / Ρ0: 0.1 to 0.3],
As examples of organic fillers other than carbon blacks, mention may be made of organic fillers of functionalized polyvinyl as described in applications WO 2006/069792, WO 2006/069793, WO 2008/003434 and WO 2008/003435.
-10For reinforcing inorganic filler, should be understood here any inorganic or mineral filler, whatever its color and its origin (natural or synthetic), also called white filler, clear filler or even non-black filler as opposed to carbon black, capable of reinforcing on its own, without other means than an intermediate coupling agent, a rubber composition intended for the manufacture of pneumatic tires, in other words capable of replacing, in its reinforcement function, a conventional carbon black pneumatic grade; such a charge is generally characterized, in a known manner, by the presence of hydroxyl groups (OH) on its surface. In other words, without a coupling agent, the inorganic filler does not make it possible to reinforce, or not sufficiently, the composition and is therefore not included in the definition of "reinforcing inorganic filler".
As reinforcing inorganic fillers, mineral fillers of the siliceous type, in particular silica (SiO2), are suitable. The silica used can be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenic silica having a BET surface as well as a CTAB specific surface, both less than 450 m 2 / g, preferably from 30 to 400 m 2 / g, in particular between 60 and 300 m 2 / g. As highly dispersible precipitated silicas (known as HDS), mention may be made, for example, of “Ultrasil” 7000 and “Ultrasil” 7005 from Degussa, “Zeosil” 1165MP, 1135MP and 1115MP from Rhodia, “ Hi-Sil ”EZ150G from the company PPG, the silicas“ Zeopol ”8715, 8745 and 8755 from the company Huber, the silicas with a high specific surface as described in application WO 03/016387.
In the present description, as regards silica, the BET specific surface is determined in a known manner by gas adsorption using the Brunauer-Emmett-Teller method described in The Journal of the American Chemical Society Vol. 60, page 309, February 1938, more precisely according to French standard NF ISO 9277 of December 1996 (multi-point volumetric method (5 points) - gas: nitrogen degassing: hour at 160 ° C - relative pressure range p / in: 0.05 to 0.17 ). The CTAB specific surface is the external surface determined according to French standard NF T 45007 of November 1987 (method B).
-11 Also suitable as reinforcing inorganic fillers are mineral fillers of the aluminous type, in particular alumina (AI2O3) or aluminum (oxide) hydroxides, or also reinforcing titanium oxides, for example described in US 6,610,261 and US 6,747,087.
The physical state in which the reinforcing inorganic filler is present is immaterial, whether in the form of powder, microbeads, granules, beads or any other suitable densified form. Of course, the term reinforcing inorganic filler is also understood to mean mixtures of different reinforcing inorganic fillers, in particular highly dispersible siliceous and / or aluminous fillers as described above.
Those skilled in the art will understand that, as an equivalent charge of the reinforcing inorganic charge described in this paragraph, a reinforcing charge of another nature, in particular organic, could be used, as soon as this reinforcing charge is covered with a inorganic layer such as silica, or else would have on its surface functional sites, in particular hydroxyls, requiring the use of a coupling agent to establish the connection between the filler and the elastomer.
To couple the reinforcing inorganic filler to the diene elastomer, use is made in a well known manner of a coupling agent (or binding agent) at least bifunctional intended to ensure a sufficient connection, chemical and / or physical, between the inorganic filler (surface of its particles) and the diene elastomer. In particular organosilanes or polyorganosiloxanes which are at least bifunctional are used.
Those skilled in the art can find examples of coupling agent in the following documents: WO 02/083782, WO 02/30939, WO 02/31041, WO 2007/061550,
WO 2006/125532, WO 2006/125533, WO 2006/125534, US 6,849,754, WO 99/09036, WO 2006/023815, WO 2007/098080, WO 2010/072685 and WO 2008/055986.
The content of coupling agent is advantageously less than 12 phr, it being understood that it is generally desirable to use as little as possible. Typically when a reinforcing inorganic filler is present, the level of coupling agent
- 12 represents from 0.5% to 15% by weight relative to the amount of inorganic filler. Its rate is preferably included in a range from 0.5 to 12 phr, more preferably included in a range ranging from 4 to 8 phr. This level is easily adjusted by a person skilled in the art according to the level of inorganic filler used in the composition.
According to the invention, when the reinforcing filler is present, the rate of reinforcing filler, preferably the reinforcing filler comprising predominantly or even exclusively carbon black, can be included in a range ranging from 20 to 200, preferably from 30 to 150 pce, preferably 40 to 100 pce, preferably 50 to 80 pce.
Epoxy resin
The composition according to the invention comprises between 1 and 30 phr of an epoxy resin.
The epoxy resins which can be used in the present invention include all the polyepoxide compounds. These can be, for example, aromatic epoxy resins, alicyclic epoxies, and aliphatic epoxies. For example, the aromatic epoxy resin may be an amine-aromatic epoxy resin. These resins are preferably novolak epoxy resins, that is to say epoxy resins obtained by acid catalysis, as opposed to resol resins, obtained by basic catalysis.
In particular, among the aromatic epoxy compounds, the epoxy resins chosen from the group consisting of 2,2 bis [4- (glycidyloxy) phenyl] propane, poly [o-cresyl glycidyl ether) -co-formaldehyde], poly are preferred. [henylglycidyl ether) -co-formaldehyde], poly [(phenylglycidyl ether) -co (hydroxybenzaldehyde glycidyl ether)] and mixtures of these compounds
More preferably, the epoxy resin is chosen from the group consisting of poly [o-cresylglycidyl ether) -co-formaldehyde], poly [o-phenylglycidyl ether) -coformaldehyde], aromatic epoxy amine resins and mixtures of these. compounds.
- 13 As an example of commercially available epoxy resins which can be used in the context of the present invention, there may be mentioned for example the epoxy resin "DEN 439" from the company Uniqema, the epoxy resin "Tris (4-hydroxyphenyl ) methane triglycidyl ether ”from Sigma-Aldrich, the cresol novolak araldite ECN 1299 epoxy resin from Hunstman.
The amount of epoxy resin is between 1 and 30 phr. Given the amine hardener used in the context of the present invention, below the minimum resin level indicated, the targeted technical effect is insufficient, while beyond the maximum indicated, there is a risk of excessive increase in stiffness and excessive penalization of hysteresis and Mooney plasticity. For all these reasons, the rate of epoxy resin is between 10 and 25 phr. More preferably, the level of resin in the composition according to the invention is between 15 and 20 phr.
Amino hardener
The epoxy resin of the composition of the invention is combined with a particular amine hardener which allows the crosslinking of the resin.
According to the invention, the amino hardener comprises at least two primary amine functions located on at least (that is to say one or more) a six-atom aromatic ring, said at least one six-atom aromatic ring comprising:
o at least one primary amine function, and o at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens and ethers, tertiary amines, thio -ethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals, so that the at least one six-atom aromatic ring does not contain a hydrogen atom located in ortho position relative to the primary amine functions, said amino hardener comprising at least one second primary amine function located on said at least one six-atom aromatic ring or on a possible second six-atom aromatic ring of said amino hardener.
In other words, the amino hardener comprises one or more six-atom aromatic rings and at least two primary amine functions located on one or distributed over several of these six-atom aromatic rings.
As is well known to those skilled in the art, the term primary amine function means an amino function in which the nitrogen atom is linked to two hydrogen atoms.
Preferably, the amine hardener comprises from 1 to 3, more preferably 1 or 2 aromatic rings with six atoms.
Preferably, the amino hardener comprises from 2 to 4, more preferably 2 primary amine functions located on at least six-atom aromatic ring of the amino hardener.
Among the halogens capable of constituting the radicals Ri, mention may be made of fluorine, chlorine, bromine or iodine atoms. Preferably, the halogens are chosen from the group consisting of chlorine and bromine atoms, more preferably the halogens are chlorine atoms.
According to a first embodiment of the present invention, the amino hardener can comprise a six-atom aromatic ring comprising:
o at least two primary amine functions, and o at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and ethers, tertiary amines, thio -ethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals, so that the said cycle does not comprise a hydrogen atom located in the ortho position with respect to the primary amine functions.
According to a second embodiment of the present invention, the amine hardener can also comprise at least two aromatic rings with six atoms, identical or different, said cycles each comprising:
o at least one primary amine function, and
- 15 o at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and ethers, tertiary amines, thioethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals, such that the said rings do not comprise a hydrogen atom located in the ortho position with respect to the primary amine functions.
According to another embodiment, the amino hardener can also comprise several aromatic rings with six atoms and at least two primary amine functions located only on one of the aromatic rings.
When the amino hardener comprises several (that is to say at least two) six-atom aromatic rings, these cycles may be the same or different. They may, for example, differ from one another by the nature of the atoms constituting said rings and / or by the number of primary amine functions located on said cycles and / or by the nature and / or the number of radicals Ri placed on said cycles and / or by the position of the primary amine functions and radicals Ri on said cycles. Preferably, when the amine hardener comprises several aromatic rings with six atoms, these cycles are identical.
As indicated above, the amino hardener comprises at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and ethers, tertiary amines, thio -ethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals. In the expression “ethers, tertiary amines, thioethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals”, a person skilled in the art understands that the terms "Substituted by linear or branched C1-C6 alkyl radicals" refer to each of the ethers, tertiary amines, thioethers, ketones, esters and amides.
Whatever the embodiment of the present invention, the amine hardener preferably comprises at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals,
- 16 halogens, and ethers, tertiary amines, thio-ethers, substituted by linear or branched C1-C6 alkyl radicals. More preferably, the amino hardener comprises at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and thioethers substituted by linear or branched alkyl radicals in C1-C6.
Whatever the embodiment of the present invention, the radicals Ri, identical or different, are chosen from the group consisting of linear or branched C1-C6 alkyl radicals. In other words, all of the radicals R 1 of the amino hardener can be linear or branched C1-C6 alkyl radicals, the linear or branched C1-C6 alkyl radicals being preferably chosen from the group consisting of methyl and ethyl radicals and propyl.
Whatever the embodiment of the present invention, the at least one aromatic ring with six atoms of the amine hardener may comprise at least two radicals Ri, identical or different, chosen from the group consisting of halogens, and ethers, tertiary amines and thioethers, substituted by linear or branched C1-C6 alkyl radicals, and at least one radical Ri chosen from the group consisting of linear or branched C1-C6 alkyl radicals.
Whatever the embodiment of the present invention, whether they are radicals Ri, or radicals of ethers, tertiary amines, thioethers, ketones, esters or amides, linear or branched C1- alkyl radicals C6 can be chosen from the group consisting of methyl, ethyl, propyl, isopropyl, isobutyl and butyl radicals. Preferably, the linear or branched C1-C6 alkyl radicals are chosen from the group consisting of methyl, ethyl and propyl radicals. More preferably, the linear or branched C1-C6 alkyl radicals are chosen from the group consisting of methyl and ethyl radicals.
Whatever the embodiment of the present invention, the atoms of the aromatic rings to the amino hardener can be carbon atoms, and optionally comprise nitrogen atoms. Preferably, all of the atoms in the aromatic rings of the amine hardener are carbon atoms. In other words,
The aromatic rings with six atoms of the amine hardener are preferably aromatic rings with six carbon atoms.
In formulas (I) to (V) presented below, it is recalled that the radicals Ri 5 can be identical or different.
According to the first embodiment of the present invention, the amino hardener can corresponds to formula (I):
(RO2-4 (NH
2/2 (I)
Preferably, according to this embodiment, the amino hardener corresponds to the formula (Π):
Ri
(Π)
According to the second embodiment of the present invention, the amine hardener can also correspond to formula (III):
in which n represents an integer ranging from 0 to 4, preferably from 1 to 3,
RI and R2, identical or different, are chosen from the group consisting of a hydrogen atom and a methyl, ethyl, isobutyl or benzyl group, preferably RI and R2 both represent a hydrogen atom.
- 18 Preferably, according to this embodiment, the amino hardener corresponds to formula (IV):
in which n represents 1 or 2, preferably 1,
RI and R2, identical or different, are chosen from the group consisting of a hydrogen atom, a methyl, ethyl, isobutyl or benzyl group, preferably RI and R2 both represent a hydrogen atom.
More preferably still, according to this embodiment, the amine hardener corresponds to formula (V):
Very preferably, according to the invention, the amino hardener is chosen from the group consisting of the compounds below and the mixtures of these compounds:
nh 2
By way of example of commercially available amino hardeners which can be used in the context of the present invention, there may be mentioned, for example, "Ethacure 100" or "Ethacure 300 from the company Albemarle," Lonzacure DETDA ", the “Lonzacure MDEA” or the “Lonzacure MCDEA” from the company Lonza.
The amount of amine hardener is between 1 and 15 phr. Below the indicated minimum, the targeted technical effect has been found to be insufficient, while beyond the indicated maximum, there is a risk of penalizing the use in the raw state of the compositions. Advantageously, the level of amine hardener is within a range ranging from 5 to 10 phr, preferably from 2 to 8 phr.
Miscellaneous additives
The rubber compositions in accordance with the invention may also comprise all or part of the usual additives usually used in elastomer compositions, such as, for example, pigments, protective agents such as anti-ozone waxes, chemical anti-ozonants, anti -oxidizers, plasticizing agents, anti-fatigue agents, reinforcing resins, a crosslinking system based either on sulfur or on sulfur and / or peroxide and / or bismaleimide donors, vulcanization accelerators, vulcanization activators.
These compositions can also contain, in addition to the coupling agents, coupling activators, agents for recovery of inorganic charges or more generally agents for aid in implementation which are capable in known manner, thanks to an improvement in the dispersion. of the filler in the rubber matrix and a lowering of the viscosity of the compositions, of improving their ability to be used in the raw state, these agents being for example hydrolysable silanes such as alkylalkoxysilanes, polyols, polyethers, primary, secondary or tertiary amines, hydroxylated or hydrolyzable polyorganosiloxanes.
When the composition according to the invention is an inner layer composition of a tire, it is advantageously devoid of antioxidant agent.
When the composition according to the invention is an internal tire layer composition, it may be devoid of plasticizer or contain less than 5 phr, preferably less than 1 phr. Alternatively and according to an equally preferred embodiment, the composition of the tire according to the invention also comprises a plasticizing agent. Preferably, this plasticizing agent is a solid hydrocarbon resin (or plasticizing resin), an extension oil (or plasticizing oil), or a mixture of the two.
Furthermore, the composition of the tire according to the invention may comprise a cobalt salt, in particular when it is used in an internal layer. The Applicants have also surprisingly found that the amine hardeners comprise at least one six-atom aromatic ring comprising at least one radical R 1 chosen from the group consisting of halogens, and ethers, tertiary amines, thioethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals, are particularly effective in compositions comprising a cobalt salt. Thus, preferably, the composition according to the invention comprises a cobalt salt and an amine hardener comprising at least one radical R 1 chosen from the group consisting of halogens, and ethers, tertiary amines, thioethers, ketones , esters and amides, substituted by linear or branched C1-C6 alkyl radicals. The cobalt salt can be chosen, for example, from the group consisting of abietates, acetylacetonates, tallates, naphthenates, resinates and mixtures of these compounds. The level of cobalt salt may for example be between 0.1 and 6 phr, for example between 0.3 and 4 phr, for example between 0.5 and 2.5 phr.
Advantageously, the composition according to the invention comprises a crosslinking system. The crosslinking system is preferably based on sulfur and a primary vulcanization accelerator, in particular an accelerator of the sulfenamide type. To this vulcanization system are added, incorporated during
-21 the first non-producing phase and / or during the productive phase, various secondary accelerators or known vulcanization activators such as zinc oxide, stearic acid, guanidine derivatives (in particular diphenylguanidine), etc. The sulfur content is preferably between 0.5 and 10.0 phr, that of the primary accelerator is preferably between 0.5 and 5.0 phr.
Any compound capable of acting as an accelerator for the vulcanization of diene elastomers in the presence of sulfur, in particular accelerators of the thiazole type and their derivatives, accelerators of the thiuram type, zinc dithiocarbamates, can be used as accelerator (primary or secondary). These accelerators are more preferably chosen from the group consisting of 2mercaptobenzothiazyle disulfide (abbreviated MBTS), N-cyclohexyl-2-benzothiazyle sulfenamide (abbreviated CBS), N, N-dicyclohexyl-2-benzothiazyle sulfenamide (abbreviated DCBS) , N-ter-butyl-2-benzothiazyl sulfenamide (abbreviated TBBS), N-terbutyl-2-benzothiazyl sulfenimide (abbreviated TBSI), zinc dibenzyldithiocarbamate (abbreviated ZBEC) and mixtures of these compounds. Preferably, a primary accelerator of the sulfenamide type is used.
Tires
The invention relates particularly to tires intended to equip motor vehicles of the tourism type, SUV (Sport Utility Vehicles), or two wheels (in particular motorcycles), or airplanes, or even industrial vehicles chosen from vans, "Heavy vehicles". - i.e. metro, bus, road transport equipment (trucks, tractors, trailers), off-road vehicles such as agricultural or civil engineering equipment -, and others.
Three types of zones can be defined within the tire:
• The radially outer zone and in contact with the ambient air, this zone essentially consisting of the tread and the external side of the tire. An external sidewall is an elastomeric layer placed outside the carcass reinforcement relative to the internal cavity of the tire, between the crown and the bead so as to completely or partially cover the area of the carcass reinforcement extending from the top to the bead.
-22 • The radially inner zone and in contact with the inflation gas, this zone generally being constituted by the layer which is impermeable to the inflation gases, sometimes called the inner sealing layer or inner liner.
• The internal zone of the tire, that is to say that between the external and internal zones. This zone includes layers or plies which are called here internal layers of the tire. These are for example carcass plies, tread underlays, plies of tire belts or any other layer which is not in contact with the ambient air or the inflation gas of the tire.
The composition defined in the present description is particularly well suited to the internal layers and to the tread of the tires.
According to a preferred embodiment of the invention, the rubber composition described above can be used in the tire as a rigid elastomer layer in at least part of the tire.
Also, in the tire according to the present invention, the composition according to the invention can be present in at least one layer chosen from an internal layer and the tread. According to the invention, the internal layer can be chosen from the group consisting of carcass plies, crown plies, rod stuffing, crown feet, decoupling layers, tread underlayment and combinations of these inner layers. Preferably, the internal layer is chosen from the group consisting of carcass plies, crown plies, rod stuffing, crown feet, decoupling layers and combinations of these internal layers.
The invention relates to the tires and semi-finished products for tires described above, to rubber articles, both in the raw state (that is to say, before baking) and in the cooked state (that is to say , after crosslinking or vulcanization).
-23 Preparation of rubber compositions
The compositions used in the treads of the invention can be manufactured in suitable mixers, using two successive preparation phases well known to those skilled in the art: a first working phase or thermomechanical kneading (so-called non-phase productive) at high temperature, up to a maximum temperature between 110 ° C and 190 ° C, preferably between 130 ° C and 180 ° C, followed by a second mechanical working phase (so-called productive phase) up to a lower temperature, typically less than 110 ° C., for example between 40 ° C. and 100 ° C., the finishing phase during which the crosslinking system is incorporated.
The process for preparing such compositions comprises for example the following steps:
a) incorporating into a diene elastomer, during a first step (called nonproductive), a reinforcing filler, by thermomechanically kneading the whole (for example in one or more times), until reaching a maximum temperature of between 110 ° C and 190 ° C;
b) cooling the assembly to a temperature below 100 ° C;
c) then incorporating, during a second (so-called productive) step, a crosslinking system;
d) knead everything up to a maximum temperature below 110 ° C.
Between 1 and 30 phr of the epoxy resin and between 1 and 15 phr of the amino hardener can be introduced, independently of each other, either during the non-productive phase (a) or during the productive phase (c) . Preferably, the epoxy resin is introduced during the non-productive phase (a) and the hardener during the productive phase (c).
By way of example, the non-productive phase is carried out in a single thermomechanical step during which, in a suitable mixer such as a conventional internal mixer, all the necessary basic constituents are first introduced (an elastomer diene, reinforcing filler, and possibly between 1 and 20 phr of an epoxy resin and between 1 and 15 phr of an amino hardener), then in a
-24second time, for example after one to two minutes of mixing, the other additives, any charge recovery agents or additional processing, with the exception of the crosslinking system. The total duration of the kneading, in this non-productive phase, is preferably between 1 and 15 min.
The first kneading step is generally carried out by incorporating the reinforcing filler into the elastomer one or more times by thermomechanically kneading. In the case where the reinforcing filler, in particular carbon black, is already incorporated in whole or in part in the elastomer in the form of a masterbatch as described for example in applications WO 97/36724 or WO 99 / 16600, it is the masterbatch which is directly kneaded and where appropriate the other elastomers or reinforcing fillers present in the composition which are not in the form of masterbatch are incorporated, as well as the additives other than the crosslinking system.
After cooling the mixture thus obtained, the crosslinking system is then incorporated into an external mixer such as a cylinder mixer, maintained at low temperature (for example between 40 ° C and 100 ° C). The whole is then mixed (productive phase) for a few minutes, for example between 2 and 15 min.
The final composition thus obtained can then be calendered, for example in the form of a sheet, a plate in particular for characterization in the laboratory, or else extruded, for example to form a rubber profile used for the manufacture of a pneumatic.
EXAMPLES
I. Measurements and tests used
1.1 Roasting time
Measurements are made at 130 ° C or 115 ° C, in accordance with French standard NF T 43-005. The evolution of the consistometric index as a function of time makes it possible to determine the toasting time of the rubber compositions, assessed in accordance with the aforementioned standard by parameter T5 (case of a large rotor), expressed in minutes, and defined as being the time required to get an increase of
-25 the consistometric index (expressed in MU) of 5 units above the minimum value measured for this index.
It will be recalled that, in a manner well known to those skilled in the art, the higher the consistometric index as a function of time, the more the crosslinking of the material will be delayed before baking.
1.2 Mooney plasticity
An oscillating consistometer is used as described in the French standard NF T 43-005 (1991). The Mooney plasticity measurement is made according to the following principle: the composition in the raw state (i.e., before baking) is molded in a cylindrical enclosure heated to 100 ° C. After one minute of preheating, the rotor turns within the test tube at 2 revolutions / minute and the torque useful for maintaining this movement is measured after 4 minutes of rotation. The Mooney plasticity (ML 1 + 4) is expressed in Mooney unit (MU, with 1 MU = 0.83 Newton.meter).
It will be recalled that, in a manner well known to those skilled in the art, the lower the Mooney plasticity, the easier the material to work. Of course, below a certain value (e.g., 20 MU, the material becomes too liquid to be usable, especially for making internal layers.
1.3 Dynamic properties
The dynamic properties G * (2%) are measured on a viscoanalyzer (Metravib VA4000), according to standard ASTM D 5992-96. The response of a sample of vulcanized composition (4 mm thick cylindrical test piece and 400 mm 2 section) is recorded, subjected to a sinusoidal stress in alternating single shear, at the frequency of 10 Hz, under normal conditions of temperature (23 ° C) according to ASTM D 1349-99, or as the case may be at a different temperature. A deformation amplitude sweep is carried out from 0.1 to 50% (outward cycle), then from 50% to 1% (return cycle). The exploited results are the complex dynamic shear modulus G *. For the return cycle, we indicate the complex dynamic shear modulus G * (2%) at 2% deformation, at 40 ° C.
-26We recall that the value of G * (2%) back to 40 ° C is representative of the rigidity of the material: the higher G * (2%) at 40 ° C, the more rigid the material.
II. Preparation of the compositions
The following tests are carried out as follows: an elastomer is introduced into an internal mixer (final filling rate: approximately 70% by volume), the initial tank temperature of which is approximately 60 ° C. diene, the reinforcing filler, between 1 and 30 phr of the epoxy resin, as well as the various other ingredients with the exception of the vulcanization system. Thermomechanical work (non-productive phase) is then carried out in one step, which lasts a total of approximately 3 to 4 min, until a maximum "fall" temperature of 165 ° C is reached.
The mixture thus obtained is recovered, it is cooled and then sulfur is incorporated, an accelerator of the sulfenamide type and between 1 and 15 phr of the amino hardener, on a mixer (homo-finisher) at 30 ° C., mixing the whole (productive phase ) for an appropriate time (for example between 5 and 12 min).
The compositions thus obtained are then calendered either in the form of plates (thickness of 2 to 3 mm) or of thin sheets of rubber for measuring their physical or mechanical properties, or extruded in the form of a profile.
III. Rubber composition tests
Eleven rubber compositions were prepared as indicated above, seven in accordance with the invention (noted below C.5 to C.ll) and four non-conforming (control composition noted below C.l to C.4). Their formulations (in pce) and their properties have been summarized in Table 1 below.
With the exception of the control composition C.l, the compositions presented in this table 1 do not cause the formation of formaldehyde during cooking.
The compositions C.2 to C.ll contain an epoxy resin (two different resins were tested) and a polyamine hardener in replacement of the couple of formophenolic resin / HMT hardener (s) contained in the conventional control composition
-27 C.l. The compositions C.5 to C.ll in accordance with the present invention contain amino hardeners, different from the amino hardeners of the control compositions C.2 to C.4.
The results on the basis of the roasting time and of G * (2%) are presented 100 with respect to the control composition C.l. The Mooney plasticity results are presented in absolute value.
Table 1
Component C.l C.2 C.3 C.4 C.5 C.6 C.7 C.8 C.9 C.10 C.ll NR (1) 100 100 100 100 100 100 100 100 100 100 100 Carbon black (2) 70 70 70 70 70 70 70 70 70 70 70 ZnO (3) 3 3 3 3 3 3 3 3 3 3 3 6PPD (4) 2.5 2.5 2.5 2.5 2.5 2.5 2.5 2.5 2.5 2.5 2.5 Stearic acid (5) 2 2 2 2 2 2 2 2 2 2 2 Sulfur 3 3 3 3 3 3 3 3 3 3 3 CBS (6) 2 2 2 2 2 2 2 2 2 2 2 Formoph resin. (7) 12 - - - - - - - - - - HMT (8) 4 - - - - - - - - - - Epoxy resin (9) - 12 - 12 12 12 16 - 12 - 12 Epoxy resin (10) - - 12 - - - - 12 - 12 - Sample hardener (il) - 4 4 - - - - - - - - Sample hardener (12) - - - 4 - - - - - - - Hardener (13) - - - - 4 - - - - - - Hardener (14) - - - - - 4 4 4 - - - Hardener (15) - - - - - - - - 4 4 - Hardener (16) - - - - - - - - - - 4 Toasting time 100 51 87 145 270 177 159 209 125 97 152 Mooney plasticity (UM) 46 77 79 62 47 39 26 38 31 39 38 G * (2%) return to 40 ° C 100 109 103 101 116 102 104 102 98 101 86
(1) Natural Rubber;
(2) Carbon black N326 (name according to standard ASTM D-1765) (3) Zinc oxide (industrial grade - company Umicore) (4) Nl, 3-dimethylbutyl-N-phenylparaphenylenediamine (Santoflex 6-PPD from the company Flexsys) (5) Stearin (“Pristerene 4931” from Uniqema) (6) N-cyclohexyl-benzothiazyl sulphenamide (Santocure CBS from Flexsys) (7) Formophenolic resin novolac (“Peracit 4536K” from Perstorp) ( 8) Hexamethylenetetramine (from Degussa)
-28 (9) Epoxy resin ("DEN 439" from the company Uniqema) (10) Epoxy resin ("Tris (4-hydroxyphenyl) methane triglycidyl ether" from the company SigmaAldrich) (11) l, 3bis (aminomethyl) cyclohexane ( from Sigma-Aldrich) (12) metaphenylene diamine from Sigma-Aldrich (13) "Lonzacure DETDA" from Lonza (14) "Ethacure 300" from Albemarle (15) "Lonzacure MDEA" from company Lonza (16) “Lonzacure MCDEA” from the company Lonza
It is noted that the use of an epoxy resin and a polyamine hardener in the compositions C.5 to C.ll in accordance with the present invention makes it possible to obtain an improved Mooney plasticity compared to the couple of phenol-resin / hardener ) HMT of the control composition C1, but also with respect to the epoxy resin / polyamine hardener couple of the control compositions C.2 to C.4. Furthermore, the compositions in accordance with the present invention also make it possible to obtain an improved roasting time or at least equivalent to that of the control composition C.l, while retaining a rigidity equivalent to that of the control compositions C.l to C.4.
In summary, the results of these tests demonstrate that the use of an epoxy resin and a particular polyamine hardener in the compositions of the invention makes it possible to obtain rubber compositions whose processability / rigidity compromise is much higher. to that of a conventional composition, or of compositions comprising other amino hardeners, not in accordance with the present invention.
This test illustrates rubber compositions which can be used in particular in internal mixtures such as carcass plies, crown plies, rod stuffing, crown feet, decoupling layers, tread underlay, in particular in carcass plies, crown plies, rod stuffing, crown feet, decoupling layers, tread underlayment, areas requiring high rigidity at low deformation.
权利要求:
Claims (21)
[1" id="c-fr-0001]
1. Rubber composition based on at least:
- a diene elastomer;
- a reinforcing filler;
- a crosslinking system;
- between 1 and 30 parts by weight per hundred parts by weight of elastomer, pce, of an epoxy resin;
- between 1 and 15 phr of an amino hardener comprising at least two primary amine functions located on at least one six-atom aromatic ring, said at least one six-atom aromatic ring comprising:
o at least one primary amine function, and o at least two radicals Ri, identical or different, chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens and ethers, tertiary amines, thio -ethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals, so that the at least one six-atom aromatic ring does not contain a hydrogen atom located in ortho position relative to the primary amine functions, said amino hardener comprising at least one second primary amine function located on said at least one six-atom aromatic ring or on a possible second six-atom aromatic ring of said amino hardener.
[2" id="c-fr-0002]
2. A rubber composition according to claim 1, in which the radicals Ri, which are identical or different, are chosen from the group consisting of linear or branched C1-C6 alkyl radicals, halogens, and ethers, tertiary amines and thioethers, substituted by linear or branched C1-C6 alkyl radicals.
[3" id="c-fr-0003]
3. A rubber composition according to claim 1 or 2, in which the radicals Ri, which are identical or different, are chosen from the group consisting of linear or branched C1-C6 alkyl radicals.
-304. A rubber composition according to claim 1 or 2, in which the at least one six-atom aromatic ring of the amino hardener comprises at least two radicals Ri, identical or different, chosen from the group consisting of
[4" id="c-fr-0004]
5 halogens, and ethers, tertiary amines and thioethers, substituted by linear or branched C1-C6 alkyl radicals, and at least one radical R 1 chosen from the group consisting of linear or branched C1-alkyl radicals C6.
5. A rubber composition according to any one of claims 1 to 4, in
10 which the linear or branched C1-C6 alkyl radicals are chosen from the group consisting of methyl, ethyl, propyl, isopropyl, isobutyl and butyl radicals, preferably from the group consisting of methyl and ethyl radicals.
[5" id="c-fr-0005]
6. A rubber composition according to any one of claims 1 to 5, in
15 wherein the at least one six-atom aromatic ring is a six-carbon aromatic ring.
[6" id="c-fr-0006]
7. A rubber composition according to any one of claims 1 to 6, in which the amino hardener corresponds to formula (I):
(81) 2-4
212 (NH (I)
[7" id="c-fr-0007]
8. Composition according to any one of claims 1 to 6, in which the amino hardener corresponds to formula (II):
(Π)
- 31
[8" id="c-fr-0008]
9. A rubber composition according to any one of claims 1 to 6, in which the amino hardener corresponds to formula (III):
in which
5 n represents an integer ranging from 0 to 4, preferably from 1 to 3,
RI and R2, identical or different, are chosen from the group consisting of a hydrogen atom and a methyl, ethyl, isobutyl or benzyl group, preferably RI and R2 both represent a hydrogen atom.
[9" id="c-fr-0009]
10. The rubber composition according to any one of claims 1 to 6 or 9, in which the amine hardener corresponds to formula (IV):
in which n represents 1 or 2, preferably 1,
15 RI and R2, identical or different, are chosen from the group consisting of a hydrogen atom, a methyl, ethyl, isobutyl or benzyl group, preferably RI and R2 both represent a hydrogen atom.
[10" id="c-fr-0010]
11. A rubber composition according to any one of claims 1 to 6, in
20 which the amino hardener corresponds to the formula (V):
(V)
-3212. Rubber composition according to any one of Claims 1 to 6, in which the amino hardener is chosen from the group consisting of the compounds below and mixtures of these compounds:
and nh 2
[11" id="c-fr-0011]
13. A rubber composition according to any one of claims 1 to 12, in
10, the level of amine hardener is in a range from 5 to 10 phr, preferably from 2 to 8 phr.
[12" id="c-fr-0012]
14. A rubber composition according to any one of claims 1 to 13, in which the epoxy resin is chosen from aromatic epoxy resins,
[13" id="c-fr-0013]
15 alicyclic epoxies and aliphatic epoxies.
15. A rubber composition according to any one of claims 1 to 13, in which the epoxy resin is chosen from the group consisting of 2,2 bis [4 (glycidyloxy) phenyl] propane, poly [o-cresylglycidyl ether) -co-formaldehyde], the
Poly [phenylglycidyl ether) -co-formaldehyde], poly [(phenylglycidyl ether) co (hydroxybenzaldehyde glycidyl ether)] and mixtures of these compounds.
- 33
[14" id="c-fr-0014]
16. A rubber composition according to any one of claims 1 to 15, in which the content of epoxy resin is between 10 and 25 phr, preferably between 15 and 20 phr.
[15" id="c-fr-0015]
17. A rubber composition according to any one of claims 1 to 16, in which the quantity of reinforcing filler is between 20 and 200 phr, preferably between 30 and 150 phr.
[16" id="c-fr-0016]
18. A rubber composition according to any one of claims 1 to 17, in which the reinforcing filler comprises carbon black, an inorganic reinforcing filler or a mixture of carbon black and inorganic reinforcing filler, preferably the reinforcing filler mostly carbon black.
[17" id="c-fr-0017]
19. A rubber composition according to any one of claims 1 to 18, in which the diene elastomer is chosen from the group consisting of natural rubber, synthetic polyisoprenes, polybutadienes, butadiene copolymers, copolymers of isoprene and mixtures of these elastomers.
[18" id="c-fr-0018]
20. A rubber composition according to any one of claims 1 to 19, further comprising between 0.1 and 6 phr of cobalt salt.
[19" id="c-fr-0019]
21. The rubber composition according to claim 20, in which the amine hardener comprises at least one radical R 1 chosen from the group consisting of halogens, and ethers, tertiary amines, thioethers, ketones, esters and amides, substituted by linear or branched C1-C6 alkyl radicals.
[20" id="c-fr-0020]
22. A finished or semi-finished rubber article comprising a rubber composition according to any one of claims 1 to 21.
[21" id="c-fr-0021]
23. A tire comprising a rubber composition according to any one of claims 1 to 21.
-3424. A tire according to claim 23, wherein the rubber composition according to any one of claims 1 to 21 is present in at least one layer chosen from among the tread and an inner layer.
25. The tire according to claim 24, in which the internal layer is chosen from the group consisting of carcass plies, crown plies, bourragestringle, crown feet, decoupling layers, tread underlayment and combinations of these inner layers.
26. A process for preparing a rubber composition according to any one of claims 1 to 21, comprising the following steps:
a) incorporating into a diene elastomer, during a first step (called nonproductive), a reinforcing filler by thermomechanically kneading the whole until reaching a maximum temperature of between 110 ° C and 190 ° C;
B) cooling the assembly to a temperature below 100 ° C;
c) then incorporating, during a second (so-called productive) step, a crosslinking system;
d) knead everything up to a maximum temperature below 110 ° C., characterized in that between 1 and 30 phr of an epoxy resin and between 1 and 15 phr of a
The amino hardener as defined in any one of claims 1 to 12 is incorporated, independently of one another, during step (a) or (c).
类似技术:
公开号 | 公开日 | 专利标题
EP2488582B1|2018-01-10|Rubber composition including an epoxide resin
EP3478759B1|2020-08-05|Rubber composition comprising an epoxidized resin and a specific amine hardener
EP2547727B1|2016-10-26|Sidewall for tire
FR3012147A1|2015-04-24|PNEUMATIC COMPRISING A COMPOSITION COMPRISING A ZINC DIACRYLATE DERIVATIVE AND A PEROXIDE
EP2877526B1|2019-12-18|Rubber composition comprising an epoxy resin and a polyimine hardener
WO2014095588A1|2014-06-26|Tyre comprising a rubber composition comprising an epoxy resin and a polyacid
EP3592808B1|2021-06-02|Tyre having a composition comprising an ethylene-rich elastomer, a peroxide and a zinc acrylate
FR3063732A1|2018-09-14|PNEUMATIC HAVING A COMPOSITION COMPRISING AN ETHYLENE-RICH ELASTOMER, A PEROXIDE AND A POLYFUNCTIONAL ACRYLATE DERIVATIVE
EP3717561B1|2022-01-05|Rubber composition with high module comprising an ultra vulcanization accelerator
WO2018109376A1|2018-06-21|Tyre provided with a composition comprising a diene elastomer, a zinc acrylate, a peroxide and a specific anti-oxidant
FR3083242A1|2020-01-03|RUBBER COMPOSITION BASED ON EPOXIDE RESIN AND AN AMINOBENZOATE DERIVATIVE
EP3703956B1|2021-12-08|Tire with innerlayer based on at least an isoprene elastomer, reinforcing resinand metallic salt
FR3074183A1|2019-05-31|HIGH MODULE RUBBER COMPOSITION COMPRISING AN EFFECTIVE SELF-RETICULATING SYSTEM
FR3108118A1|2021-09-17|RUBBER COMPOSITION BASED ON EPOXIDE RESIN AND A HIGH LATENCY HARDENER
FR3085955A1|2020-03-20|RUBBER COMPOSITION BASED ON EPOXIDE RESIN, AN AMINE HARDENER AND AN IMIDAZOLE
FR3108119A1|2021-09-17|RUBBER COMPOSITION BASED ON EPOXIDE RESIN AND A HIGH LATENCY HARDENER
FR3064640A1|2018-10-05|RUBBER COMPOSITION BASED ON REINFORCING RESIN AND AN AMINOBENZOATE DERIVATIVE
WO2013068269A1|2013-05-16|Rubber composition containing a high level of non-isoprene diene synthetic elastomer
WO2020128260A1|2020-06-25|Rubber composition comprising a polysulfide compound
EP3898263A1|2021-10-27|Rubber composition comprising a polysulfide compound
FR3052783A1|2017-12-22|REINFORCED RUBBER COMPOSITION FOR PNEUMATIC
同族专利:
公开号 | 公开日
US20190241722A1|2019-08-08|
WO2018002538A1|2018-01-04|
CN109415540B|2021-09-10|
RU2743953C2|2021-03-01|
BR112018077347A2|2019-04-02|
RU2018143450A3|2020-10-09|
FR3053344B1|2018-07-06|
EP3478759B1|2020-08-05|
EP3478759A1|2019-05-08|
RU2018143450A|2020-07-30|
CN109415540A|2019-03-01|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
WO2014016346A1|2012-07-25|2014-01-30|Compagnie Generale Des Etablissements Michelin|Rubber composition comprising an epoxy resin and a polyimine hardener|
FR2693467A1|1992-07-08|1994-01-14|Michelin & Cie|Process and composition for the use of substituted melamines as novolak resin hardeners|
FR2740778A1|1995-11-07|1997-05-09|Michelin & Cie|SILICA-BASED RUBBER COMPOSITION AND FUNCTIONALIZED DIENE POLYMER HAVING TERMINAL SILANOL FUNCTION|
EP1537908B1|1997-09-30|2012-04-04|Cabot Corporation|Elastomer composite blends and methods for producing them|
JP4234200B2|1996-04-01|2009-03-04|キャボットコーポレイション|Novel elastomer composite and method for producing the same|
FR2765882B1|1997-07-11|1999-09-03|Michelin & Cie|CARBON BLACK-BASED RUBBER COMPOSITION HAVING SILICA ATTACHED TO ITS SURFACE AND ALCOXYSILANE FUNCTIONALIZED DIENE POLYMER|
AT239737T|1997-08-21|2003-05-15|Crompton Corp|BLOCKED MERCAPTOSILANES AS A CLUTCH FOR FILLED RUBBER COMPOSITION|
CN1330961C|1997-11-28|2007-08-08|米什兰集团总公司|Reinforcing aluminium filler and rubber composition containing same|
US6098711A|1998-08-18|2000-08-08|Halliburton Energy Services, Inc.|Compositions and methods for sealing pipe in well bores|
CA2338162A1|1999-05-28|2000-12-07|Emmanuel Custodero|Diene elastomer and reinforcing titanium oxide based rubber composition for a pneumatic tyre|
AT290565T|2000-02-24|2005-03-15|Michelin Soc Tech|VULCANIZABLE RUBBER MIXTURE FOR MANUFACTURING AN AIR RIFE AND AIR TIRE CONTAINING SUCH A COMPOSITION|
CN1140570C|2000-05-26|2004-03-03|米其林技术公司|Rubber composition for use as tyre running tread|
JP5357371B2|2000-07-31|2013-12-04|コンパニーゼネラールデエタブリッスマンミシュラン|Tire tread|
CN1263792C|2000-10-13|2006-07-12|米其林技术公司|Rubber composition comprising as coupling agent polyfunctional organosilane|
CN1257171C|2000-10-13|2006-05-24|米其林技术公司|Polyfunctional organosilane as coupling agent and method for obtaining same|
FR2823215B1|2001-04-10|2005-04-08|Michelin Soc Tech|TIRE AND TIRE TREAD COMPRISING AS COUPLING AGENT A BIS-ALKOXYSILANE TETRASULFURE|
AT266669T|2001-08-06|2004-05-15|Degussa|ORGANOSILICON COMPOUNDS|
RU2004107514A|2001-08-13|2005-10-10|Сосьете Де Текноложи Мишлен |COMPOSITION BASED ON DIENE RUBBER FOR PNEUMATIC TIRES, INCLUDING SPECIAL SILICON DIOXIDE AS A REINFORCING FILLER|
FR2854404B1|2003-04-29|2005-07-01|Michelin Soc Tech|METHOD OF OBTAINING GRAFT ELASTOMER WITH FUNCTIONAL GROUPS ALONG THE CHAIN AND RUBBER COMPOSITIONS|
US7928258B2|2004-08-20|2011-04-19|Momentive Performance Materials Inc.|Cyclic diol-derived blocked mercaptofunctional silane compositions|
FR2880354B1|2004-12-31|2007-03-02|Michelin Soc Tech|ELASTOMERIC COMPOSITION REINFORCED WITH A FUNCTIONALIZED POLYVINYLAROMATIC LOAD|
FR2880349B1|2004-12-31|2009-03-06|Michelin Soc Tech|FUNCTIONALIZED POLYVINYLAROMATIC NANOPARTICLES|
FR2886304B1|2005-05-26|2007-08-10|Michelin Soc Tech|RUBBER COMPOSITION FOR PNEUMATIC COMPRISING AN ORGANOSILICIC COUPLING SYSTEM|
FR2886306B1|2005-05-26|2007-07-06|Michelin Soc Tech|PNEUMATIC RUBBER COMPOSITION COMPRISING AN ORGANOSILOXANE COUPLING AGENT|
FR2886305B1|2005-05-26|2007-08-10|Michelin Soc Tech|PNEUMATIC RUBBER COMPOSITION COMPRISING AN ORGANOSILICALLY COUPLED AGENT AND AN INORGANIC CHARGE RECOVERY AGENT|
CN1710007A|2005-07-08|2005-12-21|南京大学|Room temperature solidifed wide-temperature-range high-strength high-toughness epoxy reinforced butyronitrile adhesive|
KR20080068868A|2005-11-16|2008-07-24|다우 코닝 코포레이션|Organosilanes and their preparation and use in elastomer compositions|
US7510670B2|2006-02-21|2009-03-31|Momentive Performance Materials Inc.|Free flowing filler composition based on organofunctional silane|
FR2903416B1|2006-07-06|2008-09-05|Michelin Soc Tech|ELASTOMERIC COMPOSITION REINFORCED WITH A FUNCTIONALIZED NON-AROMATIC VINYL POLYMER|
FR2903411B1|2006-07-06|2012-11-02|Soc Tech Michelin|NANOPARTICLES OF FUNCTIONALIZED VINYL POLYMER|
FR2908410A1|2006-11-10|2008-05-16|Rhodia Recherches & Tech|PROCESS FOR THE PREPARATION OF ALCOXYSILANES SULFIDES AND NEW INTERMEDIATE PRODUCTS THEREIN|
US20120142816A1|2006-11-20|2012-06-07|Dow Global Technologies Inc|Novel epoxy hardeners with improved cure and polymers with enhanced coating properties|
FR2915202B1|2007-04-18|2009-07-17|Michelin Soc Tech|MONOMODAL COUPLED DIENIC ELASTOMER HAVING CHAIN SILANOL FUNCTION, PROCESS FOR OBTAINING THE SAME, AND RUBBER COMPOSITION CONTAINING SAME.|
FR2918064B1|2007-06-28|2010-11-05|Michelin Soc Tech|PROCESS FOR THE PREPARATION OF POLYETHER BLOCK DIENE COPOLYMER, REINFORCED RUBBER COMPOSITION AND PNEUMATIC WRAPPING.|
FR2918065B1|2007-06-28|2011-04-15|Michelin Soc Tech|PROCESS FOR THE PREPARATION OF POLYETHER BLOCK DIENE COPOLYMER, REINFORCED RUBBER COMPOSITION AND PNEUMATIC WRAPPING.|
FR2940290B1|2008-12-22|2010-12-31|Michelin Soc Tech|BLOCKED MERCAPTOSILANE COUPLING AGENT|
FR2951182B1|2009-10-14|2012-09-21|Michelin Soc Tech|RUBBER COMPOSITION COMPRISING AN EPOXY RESIN|
KR101794386B1|2010-09-24|2017-11-06|도레이 카부시키가이샤|Epoxy resin composition for fiber-reinforced composite material, prepreg, and fiber-reinforced composite material|
EP2886590B1|2012-09-28|2017-11-08|Toray Industries, Inc.|Prepreg, and carbon fiber reinforced composite material|
FR2999582B1|2012-12-17|2015-02-13|Michelin & Cie|PNEUMATIC COMPRISING A RUBBER COMPOSITION COMPRISING AN EPOXY RESIN AND A POLYACID|FR3083242B1|2018-07-02|2020-06-12|Compagnie Generale Des Etablissements Michelin|RUBBER COMPOSITION BASED ON EPOXIDE RESIN AND AN AMINOBENZOATE DERIVATIVE|
FR3085955B1|2018-09-17|2020-09-11|Michelin & Cie|COMPOSITION OF RUBBER BASED ON EPOXIDE RESIN, AN AMINE HARDENER AND AN IMIDAZOLE|
FR3108118A1|2020-03-10|2021-09-17|Compagnie Generale Des Etablissements Michelin|RUBBER COMPOSITION BASED ON EPOXIDE RESIN AND A HIGH LATENCY HARDENER|
FR3108119A1|2020-03-10|2021-09-17|Compagnie Generale Des Etablissements Michelin|RUBBER COMPOSITION BASED ON EPOXIDE RESIN AND A HIGH LATENCY HARDENER|
法律状态:
2017-06-21| PLFP| Fee payment|Year of fee payment: 2 |
2018-01-05| PLSC| Search report ready|Effective date: 20180105 |
2018-06-26| PLFP| Fee payment|Year of fee payment: 3 |
2020-03-13| ST| Notification of lapse|Effective date: 20200206 |
优先权:
申请号 | 申请日 | 专利标题
FR1656142A|FR3053344B1|2016-06-30|2016-06-30|RUBBER COMPOSITION COMPRISING AN EPOXY RESIN AND A SPECIFIC AMINE HARDENER|
FR1656142|2016-06-30|FR1656142A| FR3053344B1|2016-06-30|2016-06-30|RUBBER COMPOSITION COMPRISING AN EPOXY RESIN AND A SPECIFIC AMINE HARDENER|
PCT/FR2017/051749| WO2018002538A1|2016-06-30|2017-06-29|Rubber composition comprising an epoxide resin and a specific amine hardener|
BR112018077347A| BR112018077347A2|2016-06-30|2017-06-29|rubber composition comprising an epoxy resin and a specific amine hardener|
EP17740450.6A| EP3478759B1|2016-06-30|2017-06-29|Rubber composition comprising an epoxidized resin and a specific amine hardener|
RU2018143450A| RU2743953C2|2016-06-30|2017-06-29|Composition of rubber containing epoxy resin and amine hardener|
US16/314,100| US20190241722A1|2016-06-30|2017-06-29|Rubber composition comprising an epoxide resin and a specific amine hardener|
CN201780041156.6A| CN109415540B|2016-06-30|2017-06-29|Rubber composition comprising an epoxy resin and a specific amine hardener|
[返回顶部]