专利摘要:
The present invention relates to a process for the preparation of rigid mineral and porous foams and their applications as refractory thermal insulating material in construction or industry.
公开号:FR3049597A1
申请号:FR1652756
申请日:2016-03-30
公开日:2017-10-06
发明作者:Corfec Yves Le
申请人:Ipsiis;
IPC主号:
专利说明:

Process for the preparation of porous inorganic rigid foams and their uses
The present invention relates to a process for the preparation of rigid mineral and porous foams and their applications as refractory thermal insulating material in construction or industry.
The depletion of fossil fuels and primary resources requires the development of new thermal insulation materials that are effective and environmentally acceptable. The materials currently used in building insulation are effective but have weaknesses. Some materials, such as polyurethane foam, polyester wadding, expanded or extruded polystyrene, or insulating materials of plant or animal origin, are flammable. Some of the insulating materials currently available on the market can be harmful to health or the environment. Others do not improve fire resistance or fire safety and may have recycling constraints.
In recent years, the focus of development of new thermal and refractory insulation materials has shifted to mineral-based materials known to be refractory. Several production methods have been proposed in the literature for the production of light mineral materials, often in the form of rigid foam.
The application WO 2007/043022 describes a process for manufacturing a porous refractory ceramic material from an aqueous suspension of ceramic powders into which a granular organic agent is added as a blowing agent and a foaming agent. After stabilization, this foam undergoes a first heat treatment at a temperature between 50 ° C and 110 ° C and a second heat treatment at a temperature above 1500 ° C. This heat treatment makes it possible to calcine the porogenic agents in order to generate the porosity of the material.
The application WO 2008/146320 describes a thermal and acoustic insulating material. This material has a cellular structure comprising ceramic fibers, such as glass wool or mineral wool and is formed by a foam emulsion comprising ceramic fibers, at least one silicate binding agent and at least one foaming agent organic emulsifier. The length of the fibers used is preferably from 0.2 cm to 5 cm. The aforesaid emulsion first undergoes a first heat treatment from 70 ° C. to 120 ° C. in order to consolidate the structure of the foam and to obtain a solid body. Said solid body then undergoes a second heat treatment at high temperature, in particular from 400 ° C to 800 ° C to remove the organic components present in said solid body and obtain the final material.
These materials are refractory and effective in terms of thermal insulation. However, their production is energetically expensive because of the need for high temperature heat treatment.
There is therefore a need for healthy materials that can be obtained by a simple and inexpensive process, possessing excellent insulating and refractory character, and low production cost, for use in building construction and building. industry.
The present invention therefore aims to overcome the aforementioned drawbacks by proposing a new process for preparing rigid foams mineral and porous.
Said process comprises the following steps: (i) the preparation of an aqueous suspension comprising or consisting of - 35% -60% of water by total weight of the aforesaid suspension, - 5-35% by total weight of the aforesaid suspension an alkali metal silicate, an alkali metal aluminate, or mixtures thereof, - 30-60% by total weight of the aforesaid suspension of mineral particles insoluble in the aforesaid suspension, - 0-2% by total weight of the aforesaid suspension of mineral or organic fibers, - 0.3-10%, especially 0.3-5%, by total weight of the aforesaid suspension of at least one foaming agent of animal or plant origin, natural or synthetic - optionally at least one texturing agent, - optionally, at least one functional molecule, and - optionally, a surfactant different from the foaming agent used in said suspension, (ii) dispersing a gas in the aforesaid suspension to obtain a stable wet foam; (iii) curing the wet foam obtained at the end of step (ii) to obtain said rigid foam. The invention proposes a process that is easy to implement and ecologically responsible. The method of the invention makes it possible to valorize natural resources and recycled materials in a production with very low marginal cost.
The porous rigid foams obtained by the process of the present invention possess excellent thermal and / or sound insulating properties, good heat capacity, and are capable of withstanding high temperatures (above 1000 ° C. or even 1500 ° C. depending on the raw materials chosen).
The rigid foams obtained by the process of the invention have an open double porosity. The porosity of these materials is attributed both to the gas bubbles initially constituting a stable wet foam and to the removal of the water initially present in this wet foam, and also to the entrained air entrainments on the micrometer particles of the suspension, which produce micropores and nanopores. According to the invention, the dispersed gas generates pores with a size of the order of ten micrometers, while pores of the order of one hundred nanometers are produced during the evaporation of water.
The method is particularly favorable in terms of energy because the curing of the wet foam does not require any heat treatment at a high temperature prior to obtaining a material having satisfactory insulating and refractory characteristics.
Another advantage of the process of the present invention results from the possibility of a preparation prior to the use of the aqueous suspension. The aqueous suspension of step (i) can be stored for several months without noticeable alterations in properties and potential.
According to the invention, an alkali metal silicate is a binder precursor for the aggregation of mineral particles. As an example of alkali metal silicate, there may be mentioned sodium silicate, magnesium, or potassium. As an example of alkali metal aluminate, there may be mentioned sodium aluminate, magnesium, or potassium.
In general, the sodium silicate used in the invention has an SiO 2 / Na 2 O molar ratio of between 2 and 4. The choice of this ratio influences the pH of the suspension obtained in the aforesaid step (i): a ratio lower than 2.8 leads to a strongly alkaline suspension; a ratio higher than 2.9 allows, on the other hand, to produce a suspension closer to neutrality.
Too high a pH of the aqueous suspension of step (i) can lead to coagulation of the foaming agents of this suspension and therefore to the formation of macroporosities. Those skilled in the art will be able to adapt the concentration of the silicate solution and / or aluminate of alkali metal depending on the nature and the surface state of the particles and / or fibers used and according to the mechanical characteristics sought for the finished material.
Advantageously, the weight ratio of alkali metal silicate or alkali metal aluminate or mixtures thereof in an aqueous suspension of step (i) is 5 to 15%.
In a particular embodiment, the alkali metal silicate can be produced in situ directly in the aqueous suspension according to conventional methods known to those skilled in the art.
In the context of the present invention, the minerals as raw material used to obtain the aqueous suspension are in particulate form.
By "particle" is meant powders having a median grain diameter of 1 to 100 μm, ideally in the range of 5 to 50 μm. By way of example, the mineral particles that may be used in the context of the invention are the particles of one or more minerals chosen from the group comprising glasses, bricks, sandstones, feldspars, ceramics, clays, dehydroxylated clays. , carbonates, phosphates, metal oxides, borides of metals or silicon, carbides of metals or silicon, slags, ashes and silico-aluminous mixtures, nitrides, silica microballoons or cenospheres, silicates such as calcium silicate, carbon such as graphite or coal, kaolin, metakaolin, talc, zircon, chromite, boron or sulfur phosphide, elemental boron, titanium dioxide, apatite, hydroxyapatite, pozzolan, alumina, anthracite, olivine, magnesite, silica, fumed silica, or silica fume.
The raw materials in particulate form are insoluble in the aqueous suspension obtained in step (i).
The mineral particles used in step (i) of the process of the invention may be recycled materials.
It should be noted that these minerals can play a functional role in addition to their structural role within a rigid foam obtained by the process of the invention and confer on the latter possibly additional functions. For example, some minerals are electrically conductive and can absorb electromagnetic waves.
The aqueous suspension of step (i) may also comprise between 0 and 2% by total weight of the aqueous suspension of the mineral or organic fibers to reinforce or arm the rigid foam obtained by the process of the invention. Said fibers may be synthetic or natural mineral or organic fibers. These fibers can be dispersed in the aqueous suspension or in the stable wet foam before solidification. The fibers used in the process of the invention have a length greater than 10 μm and less than 500 μm, and a length / diameter ratio greater than 3, and a weight ratio of less than 1% relative to the final mass of said rigid foam.
According to the invention, the foaming agent used in step (i) of the process is one or the mixture of several foaming agents of animal or plant origin, natural or synthetic. These foaming agents are chosen in particular from the group comprising egg white, lecithins, and optionally hydrolysed natural or synthetic proteins, such as serum proteins, in particular albumin, caseins, whey proteins and proteins. plants of the Fabaceae and Poaceae family, halogenated proteins, or a mixture of the above foaming agents.
These foaming agents may be a natural product obtained by the extraction or purification from an animal or a plant or a synthetic compound having the chemical structure or the amino acid sequence identical to that of a natural product extracted or purified from an animal or plant.
In a particularly advantageous embodiment, the foaming agent used in step (i) of the process of the invention is egg white or albumin.
According to the invention, the aqueous suspension of step (i) may further comprise a surfactant different from the foaming agent used in said suspension, which advantageously reduces the amount of foaming agent used.
Said surfactant may be a conventional surfactant, advantageously halogenated surfactants, sucroesters, fatty acids and alcohols.
Advantageously, when said surfactant is present in the suspension, its proportion by weight is between 0.3 and 10%, especially between 0.3 and 3% by total weight of this suspension.
The aqueous suspension of step (i) may further comprise a texturizing agent, which makes it possible to stabilize, fluidify, improve the texture of the wet foam and optimize the consumption of surfactant by adapting the characteristics of the porosities to the needs. In another suitable manner, said texturizing agent is a conventional thickener and may be selected from cellulose derivatives, gums, agar-agar, gelatins, alginates, carrageenans, pectin, and beet sugars. or sugar cane.
Examples of cellulose derivatives are carboxymethylcellulose, hydroxypropylmethylcellulose and hydroxyethylcellulose. As an example of gums, there may be mentioned natural gums, such as guar gum, locust bean gum, xanthan range, or gellan gum.
Advantageously, the amount of texturing agent in said aqueous suspension is between 0 and 0.3% by weight of said suspension.
The aqueous suspension of step (i) may further comprise a functional molecule.
For the purposes of the invention, the term "functional molecule" means an element whose presence in a rigid foam obtained according to the process of the invention is not essential, but makes it possible to confer on said foam functionalities enriching the properties of thermal, refractory and acoustic insulation shared by all the rigid foams obtained by the process of the invention.
In a particular embodiment of the invention, the aqueous suspension of step (i) comprises at least one functional molecule chosen from a catalyst, a dye, a compound possessing gas sorption or wave absorption properties. electromagnetic.
Some functional molecules may also be incorporated into the wet foam obtained in the above-mentioned step (ii).
In another advantageous embodiment, the above-mentioned suspension in step (i) consists of: 35-40% of water by total weight of the aforesaid suspension, 5-35% by total weight of the aforesaid suspension at least one alkali metal silicate, an alkali metal aluminate, or mixtures thereof, - 30-37% by total weight of the aforesaid suspension of mineral particles and 0-2% by total weight of the aforesaid suspension of mineral fibers, 0.3-10%, especially 0.3-5% by total weight of the above suspension of a foaming agent chosen from egg white, serum proteins, in particular albumin, caseins, whey proteins, plant proteins of the family Fabaceae and Poaceae, halogenated proteins, or a mixture of the above foaming agents.
In another advantageous embodiment, the suspension mentioned above in step (i) consists of: - 45-55% total water of the suspension, - 10-35% by total weight of the aforesaid suspension at least one alkali metal silicate, an alkali metal aluminate, or mixtures thereof, - 30-40% by total weight of the aforesaid suspension of mineral particles and 0-2% by total weight of the aforesaid suspension of mineral fibers, 0.3-10%, especially 0.3-5% by total weight of the above suspension of a foaming agent chosen from egg white, serum proteins, in particular albumin, caseins, whey proteins, plant proteins of the family Fabaceae and Poaceae, halogenated proteins, or a mixture of the above foaming agents, and - 0-0.2% by total weight of the aforesaid suspension of at least one agent texturing.
In another advantageous embodiment, the above-mentioned suspension in step (i) consists of: 35-60% of water by total weight of the aforesaid suspension, 5-35% by total weight of the aforesaid suspension at least one alkali metal silicate, an alkali metal aluminate, or mixtures thereof, - 30-50% by total weight of the aforesaid suspension of mineral particles and 0-2% by total weight of the aforesaid suspension of mineral fibers, - 0.3-10%, especially 0.3-5%, by total weight of the above suspension of a foaming agent chosen from egg white, serum proteins, in particular albumin, caseins , whey proteins, plant proteins of the Fabaceae and Poaceae family, halogenated proteins, or a mixture of the above foaming agents, - 0-0.3% by total weight of the aforesaid suspension of at least one agent texturizer, and - 0.3-10% by total weight of the aforesaid suspension of at least one surfactant.
The aforesaid aqueous suspension can be prepared quickly and before use and can be easily preserved provided it is protected from CO2 in order to prevent any carbonation. Step (ii) of the process of the invention makes it possible to produce a wet foam, a step determining the shape and porosity of the material obtained by the process of the invention.
The ability to produce a porous composite structure is essential for the physicochemical properties of the materials obtained by the process of the invention.
The gas bubbles are dispersed in the aqueous suspension obtained in step (i) by any conventional method.
The dispersion of the gas in the suspension generating the micropores, the control of the gas supply and the expansion energy makes it possible to regulate the size of this type of pores and to adapt it to the stakes By way of example, the gas used in the above step (ii) may be air, argon, nitrogen, or any other inert gas or mixtures thereof, carbon dioxide, or mixtures of at least one gas inert with the dioxide of carbon. Carbon dioxide initiates, if it is present, the hardening process. Those skilled in the art will be able to choose the gas according to their affinity for water, silicates, aluminates or according to their own physical properties.
The hardening of the stable wet foam obtained at the end of step (ii) can be implemented by several methods known in the prior art, in particular: by dehydration, by heating, by injection of CO2, by addition of dry matter powder or metal powder, or - by addition of acids, organic esters, alkylene carbonates, or acetic esters.
For the purposes of the present invention, the terms "hardening", "solidification" or "stiffening" are interchangeable. By way of example, this stable moist foam may be cured thermally, in particular by heating at a temperature between 30 ° C. and 200 ° C., which leads to the coagulation of the constituents of said wet foam, such as foamy agents. protein, and the formation of silica in solid form by evaporation of the water contained in said wet foam.
Heating the foamy mixture can be implemented by any conventional method, including a microwave oven.
This mode of hardening can be easily integrated into an industrial process.
The hardening of a wet foam by heating with a microwave oven, to obtain a rigid foam "ready for use" can take place very quickly, of the order of a few tens of seconds, which allows industrial production on site or even obtaining a rigid foam having a desired three-dimensional structure using known technologies, for example "3D printing".
The hardening can also be implemented by spontaneous coagulation, following the pH modification linked to the partial solubilization of CO2, the latter possibly being the atmospheric CO2 initially trapped in the aqueous suspension or as the hardening progresses, or CO2 injected into the wet foam before or during stabilization.
Coagulation can also be triggered by adding finely divided dry matter powder or alkali metal powder to the unstabilized foamy mixture. This coagulation is the result of the combined increase of the SiO 2 / Na 2 O ratio and the solid matter by addition of silicon, ferro-silicon, magnesium, aluminum to the stable wet foam or by direct addition of the sodium silicate, which leads to exothermic physicochemical reaction which dehydrates the foamy mixture.
The hardening can also be carried out by supplying weak acids or organic esters, such as polyalcohol esters, mono-, di- or tri-esters of glycerol, in particular mono-, di-, or glycerol triacetate, or alkylene carbonates, such as propylene carbonate or ethylene carbonate, or acetic esters, such as ethyl acetate. These components can be made to the wet foam.
The solidification of the foam by adding CO2, acids or esters may require the implementation of larger amounts of alkali metal silicates. Those skilled in the art will be able to adjust the amount of alkali metal silicates used according to its chosen stabilization mode.
In a particular embodiment, said method is implemented by continuous flow production. Continuous flow production can be implemented by any type of conventional device.
The rigid foams from the process of the invention have a low thermal conductivity, namely about 40-60 mW / m / K, which allows them to be used as building material, external thermal insulating material and / or building, in industry, geotechnical applications, transportation, mining, engineering structures, exploration or oil and gas production.
Due to the high porosity of the rigid foams obtained by the process of the invention, these foams can also be used as exterior and / or interior building insulation material.
As the hardening of stable wet foams by diffusion of CO2 possibly present in the foam or diffusion of atmospheric CO2, the rigid foams obtained can be used as thermal insulation foam and / or phonic hardening delayed but spontaneous.
This property makes it possible to avoid an additional stabilization step by other means, when this spontaneous hardening is compatible with the intended application, such as the case of certain applications to the building.
In a particular embodiment, the invention relates to the use of rigid foams obtained by the process described above as a vacuum insulation support by applying an impermeable envelope to the rigid foam panels of the invention. The latter then ensure the obtaining of an empty volume of air.
A porous rigid foam produced by the process of the invention can also be used as a heat storage element in the manufacture of a heat exchanger or well, because of its very good heat capacity over a wide temperature range and of its porous character.
Another advantageous aspect of the rigid foams produced by the process of the invention is that they are resistant to very high temperature.
These rigid foams can be used as a fire-resistant material or a material for protection against fire, heat, or radiation, especially infrared radiation, or as a material for the manufacture of industrial elements that require resistance to high temperature.
According to one embodiment of the invention, said rigid foams can be used for the manufacture of composites.
In particular, the rigid foams obtained by the process of the invention can be used as a material for the manufacture of molds, in particular high-temperature refractory molds, more particularly, foundry molds or electrolysis molds.
According to a particular embodiment, the rigid foams of the invention can be used as a support for pyrolysis.
In a particular embodiment, the rigid foams of the invention can be used as a precursor for ceramic foams.
Another particular embodiment of the invention relates to the use of a stable wet foam obtained at the end of step (ii) of the process of the invention, which is not yet hardened and is still in the form of plastic, like foam for the fight against fire.
This wet and stable foam, in contact with fire or by diffusion of atmospheric CO2, is solidified and converted into refractory rigid foam, nonflammable and then limits the spread.
The rigid foams produced by the process of the invention can also be used as nonflammable core material of composite materials.
In addition, the low density of the rigid foams of the invention related to their porous nature allows them to be used as a conditioning foam or protection against shocks, or as a cavity inerting material and design of explosion-proof barriers.
Another particular embodiment is the use of the rigid foams of the invention as a buoyancy reserve.
According to another particular embodiment, the rigid foams of the invention can be used as building material, lamination support, core or binder for the constitution of composite or laminated elements.
The cellular structure and the physico-chemical properties of certain constituents of the rigid foams of the invention also give them specific applications.
Thus, in a particular embodiment, the rigid foams produced by the process of the invention are used as air conditioning material or liquid or gas treatment by filtration or sorption.
According to another particular embodiment, the invention relates to the use of a rigid foam of the invention as a catalyst support, either thanks to the minerals contained in said foam and functioning as a catalyst; either by adding a catalyst as a functional molecule in the suspension obtained according to the aforesaid step (i).
Another aspect of the use of a rigid foam obtained according to the method of the invention relates to the use of a foam on the surface of which is deposited a fuel, as infrared radiating material. The invention also relates to the use of an electronically conductive rigid foam previously described as an electromagnetic shielding material. The invention is further illustrated by the following examples and the figures below.
FIGS. 1A, 1B and 1C show the microstructure of the rigid inorganic foams obtained by the method of the invention observed by scanning electron microscopy. The open double porosity of the rigid foam is observed. This foam has micropores with a size of 50 to 500 μm and nanopores with a size of 50 to 500 nm. Figure IA illustrates the micropores of the rigid foam. Figure 1B illustrates in more detail the walls of the micropores. Figure IC shows that the walls are made of nanopores.
FIGS. 2A and 2B respectively illustrate the structure of a stable wet foam (FIG. 2A) and that of a rigid foam (FIG. 2B) obtained by the method of the invention.
Examples 1. Refractory property of the rigid foams of the invention
Rigid foams in the form of a thick test piece of 6 × 15 × 15 cm are obtained according to the process of the invention.
Flame resistance tests were carried out on these rigid foams, one side of which was exposed to the flame of more than 1500 ° C, produced by an electro-burner, for several tens of minutes.
These tests show that the integrity of the test piece has been maintained and that a temperature gradient of 200 ° C / cm is easily obtained.
The thermal shock resistance capability and the dimensional stability of these foams are also analyzed.
The thermal shock resistance capacity is tested by high alloy steel casting at 1400 ° C on a rigid foam of the invention.
The dimensional stability of a foam was tested by holding at 1050 ° C for 2 hours. During this test, the verification of the absence of any significant modification of the macrostructure is made.
These experiments show that the rigid foams of the invention are very resistant to thermal shocks and have a very good dimensional stability. 2. Thermal conductivity test
Various thermal conductivity measurements have been made on the aforementioned rigid foams obtained by the method of the invention. The method used is that described by International Standard ISO 22007-2: 2015. It is based on the use of a transient planar sensor that provides access to thermal conductivity. The measured thermal conductivities are of the order of 55 mW / mK for densities of 180 kg / m3.
权利要求:
Claims (10)
[1" id="c-fr-0001]
A process for preparing a rigid, inorganic and porous foam, comprising the following steps: (i) the preparation of an aqueous suspension comprising or consisting of - 35% -60% water by total weight of the aforesaid suspension 5-35% by total weight of the above suspension of an alkali metal silicate, an alkali metal aluminate, or mixtures thereof, 30-60% by total weight of the aforesaid suspension of insoluble mineral particles in the aforesaid suspension, - 0-2% by total weight of the aforesaid suspension of mineral or organic fibers, - 0.3-10%, especially 0.3-5%, by total weight of the aforesaid suspension of at least a foaming agent of animal or plant origin, natural or synthetic, - optionally at least one texturing agent, and - optionally, at least one functional molecule, and - optionally, a surfactant different from the foaming agent used in said suspension, ( (ii) the dispersion of a gas in the aforesaid suspension for a stable wet foam; (iii) curing the wet foam obtained at the end of step (ii) to obtain said rigid foam.
[2" id="c-fr-0002]
2. Process for preparing a foam according to claim 1, characterized in that the mineral particles are the particles of one or more minerals selected from the group consisting of glasses, bricks, sandstones, feldspars, ceramics, clays, dehydroxylated clays. , carbonates, phosphates, metal oxides, borides of metals or silicon, carbides of metals or silicon, slags, ashes and silico-aluminous mixtures, nitrides, silica microballoons or cenospheres, silicates such as calcium silicate, carbon such as graphite or coal, kaolin, metakaolin, talc, zircon, chromite, boron or sulfur phosphide, elemental boron, titanium dioxide, apatite, hydroxyapatite, pozzolan, alumina, anthracite, olivine, magnesite, silica, fumed silica, or silica fume.
[3" id="c-fr-0003]
3. A method for preparing a mineral foam according to claim 1 or 2, characterized in that said foaming agent is selected from egg white, lecithins, and natural or synthetic proteins optionally hydrolysed, such as serum proteins. including albumin, caseins, whey proteins, plant proteins of the family Fabaceae and Poaceae, halogenated proteins, or a mixture of the above foaming agents.
[4" id="c-fr-0004]
4. Process for the preparation of a mineral foam according to any one of claims 1 to 3, characterized in that said functional molecule is chosen from a catalyst, a dye, a compound having gas-absorbing or absorption properties. electromagnetic waves.
[5" id="c-fr-0005]
5. Process for preparing a mineral foam according to any one of claims 1 to 4, characterized in that said texturing agent is selected from cellulose derivatives, gums, agar-agar, gelatins, alginates , carrageenans, pectin, and beet or sugarcane sugars.
[6" id="c-fr-0006]
6. Process for preparing a mineral foam according to any one of claims 1 to 5, characterized in that said surfactant is selected from a halogenated surfactant, sucroesters or fatty acids and alcohols.
[7" id="c-fr-0007]
7. A method for preparing a mineral foam according to any one of claims 1 to 6, characterized in that said wet foam is cured: - by dehydration, - by heating, - by CO2 injection, - by adding powder dry matter or metal powder, or - by addition of acids, organic esters, alkylene carbonates, or acetic esters.
[8" id="c-fr-0008]
8. Process for preparing a mineral foam according to any one of claims 1 to 7, characterized in that said process is implemented by continuous flow production.
[9" id="c-fr-0009]
9. Use of a foam obtained according to any one of claims 1 to 8 as a building material, thermal insulating material and / or phonic, in the building, industry, geotechnical applications, transportation, mines, buildings and buildings. engineering structures, exploration, oil and gas production; as a fire-resistant material or a material for protection against fire, heat or radiation; as a material for the manufacture of molds, especially molds and refractories at high temperature; as a precursor for ceramic foams; as conditioning foam or impact protection; as a building material, laminating support, core or binder for forming composite or laminated elements; as air conditioning material, treatment of liquids or gases by filtration or sorption; as a heat storage element in the manufacture of exchanger or heat sink; as a catalyst support, said foam being obtained from a said suspension optionally comprising at least one catalyst as a functional molecule; as electromagnetic shielding material, said foam being obtained from said suspension comprising electrically conductive inorganic particles or metallic or mineral powders made conductive; as a buoyancy reserve; as an explosion-proof and cavity-inert material.
[10" id="c-fr-0010]
10. Use of a wet foam obtained at the end of step (ii) defined according to claim 1 as fire fighting foam.
类似技术:
公开号 | 公开日 | 专利标题
EP3225607A1|2017-10-04|Process for the preparation of solid porous mineral foams and their uses
EP3006417A1|2016-04-13|New porous rigid mineral foams and their uses
Bai et al.2017|High-porosity geopolymer foams with tailored porosity for thermal insulation and wastewater treatment
FR2922543A1|2009-04-24|PROCESS FOR THE PREPARATION OF A CONTROLLED POROSITY-BASED GEOPOLYMER, THE GEOPOLYMER THUS OBTAINED AND ITS DIFFERENT APPLICATIONS
Shao et al.2008|Novel method for fabrication of silicon nitride/silicon oxynitride composite ceramic foams using fly ash cenosphere as a pore‐forming agent
RU2403230C1|2010-11-10|Method of obtaining granular heat insulating material
JP5466801B2|2014-04-09|Inorganic hollow fine particles
Li et al.2016|Effects of a two-step heating process on the properties of lightweight aggregate prepared with sewage sludge and saline clay
Papa et al.2016|Insights into the macroporosity of freeze-cast hierarchical geopolymers
CN112334429A|2021-02-05|Particle-stabilized foams using sustainable materials
KR19990087722A|1999-12-27|Insulation building materials
Schelm et al.2019|Hierarchical‐Porous Ceramic Foams by a Combination of Replica and Freeze Technique
RU2563866C1|2015-09-20|Method to produce fine-grain glass foam ceramics
EP1641726B1|2008-05-14|Thermal and/or acoustic insulation materials made from silica and methods for production thereof
Shi et al.2022|The roles of cenosphere in ultra-lightweight foamed geopolymer concrete |
EP2855998B1|2017-12-27|High performance thermal insulation products
WO2013007958A1|2013-01-17|High-performance thermal insulation materials
Verma et al.2013|Processing of silica foam using steam heating and its characterization
WO2015144882A1|2015-10-01|Method for producing a macroporous and mesoporous geopolymer, with controlled porosity
Ketov et al.2021|Recycling of rice husks ash for the preparation of resistant, lightweight and environment-friendly fired bricks
WO2013156722A1|2013-10-24|Porous material for lining a building brick
Li et al.2021|Foaming performance of the closed–pore foamed ceramics using silicon nitride as a foaming agent and sodium tetraborate as a modifier of foaming
US20210170476A1|2021-06-10|Expandable aggregate mixture for molds, mold, and method for manufacturing mold
WO2019122678A1|2019-06-27|Geopolymer foam and method of producing same
Miryuk2018|Porous magnesia compositions of a combined structure
同族专利:
公开号 | 公开日
EP3225607B1|2021-05-05|
EP3225607A1|2017-10-04|
FR3049597B1|2021-04-16|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
JP2001072480A|1999-08-31|2001-03-21|Hitachi Chem Co Ltd|Heat-insulative coating composition|
EP1164179A2|2000-06-16|2001-12-19|Rex Industrie-Produkte Graf von Rex GmbH|Fibre-free, incombustible, foamed insulation and fire-protecting material and method for its manufacture|
EP1945593A2|2005-10-12|2008-07-23|Institut National Interuniversitaire des Silicates, Sols et Materiaux , a.s.b.l.|Method for producing a porous ceramic material and material obtained thereby|
WO2008146320A2|2007-05-25|2008-12-04|Fincantieri Cantieri Navali Italiani S.P.A.|Thermal and acoustic insulating material|
EP3006417A1|2014-10-09|2016-04-13|Glaztec'h|New porous rigid mineral foams and their uses|
CN107903082A|2017-11-21|2018-04-13|安徽北马科技有限公司|A kind of preparation method of cement foam concrete|
CN108425245B|2018-04-08|2020-08-14|美雅服饰有限公司|Preparation method of flame-retardant cotton fiber|
CN109437802B|2018-12-14|2021-04-27|中北大学|Sulphoaluminate cement assembled integrated inner wall and preparation method thereof|
CN109467372B|2018-12-14|2021-04-06|中北大学|Sulphoaluminate cement foaming insulation board and preparation method thereof, and assembled integrated insulation wall and preparation method thereof|
CN110423134A|2019-08-07|2019-11-08|东北大学|It is a kind of using gold ore tailing as foamed ceramics of raw material and preparation method thereof|
CN111995340A|2020-08-26|2020-11-27|盐城工学院|Regenerated fine aggregate aerated building block with electromagnetic wave absorption performance and preparation method thereof|
CN112778021A|2021-03-26|2021-05-11|浙江忠信新型建材股份有限公司|Porous light plastering gypsum and using method thereof|
法律状态:
2017-03-27| PLFP| Fee payment|Year of fee payment: 2 |
2017-10-06| PLSC| Search report ready|Effective date: 20171006 |
2018-03-28| PLFP| Fee payment|Year of fee payment: 3 |
2020-03-27| PLFP| Fee payment|Year of fee payment: 5 |
2021-03-29| PLFP| Fee payment|Year of fee payment: 6 |
优先权:
申请号 | 申请日 | 专利标题
FR1652756A|FR3049597B1|2016-03-30|2016-03-30|PROCESS FOR PREPARING RIGID POROUS MINERAL FOAMS AND THEIR USES|FR1652756A| FR3049597B1|2016-03-30|2016-03-30|PROCESS FOR PREPARING RIGID POROUS MINERAL FOAMS AND THEIR USES|
EP17162369.7A| EP3225607B1|2016-03-30|2017-03-22|Process for the preparation of solid porous mineral foams|
[返回顶部]