专利摘要:
The invention relates to a method for determining a suitable energy for implantation of at least two atomic species in a donor substrate (30) to create an embrittlement zone (31) defining a single-crystal semiconductor monocrystalline layer (32). transfer onto a recipient substrate (10), comprising the following steps: (i) forming a dielectric layer on the donor substrate (30) and / or the receiving substrate (10), (ii) co-implantation of said species into the donor substrate (30), (iii) bonding the donor substrate (30) to the recipient substrate (10), (iv) detaching the donor substrate (30) along the embrittlement zone (31) so as to transfer the layer (32) semiconductor monocrystalline and recovering a remainder (34) of the donor substrate, (v) inspecting the peripheral ring of the remainder (34) of the donor substrate or of the receiving substrate (10) on which the semiconductor monocrystalline layer ( 32) was transferred to step ( iv), (vi) if said ring has zones transferred to the receiving substrate, determining that the implantation energy of step (ii) is too high, (vii) if said ring does not have zones transferred to the receiving substrate, determining that the implantation energy of step (ii) is suitable.
公开号:FR3048548A1
申请号:FR1651747
申请日:2016-03-02
公开日:2017-09-08
发明作者:Ludovic Ecarnot;Mohamed Nadia Ben;Carine Duret
申请人:Soitec SA;
IPC主号:
专利说明:

METHOD FOR DETERMINING APPROPRIATE ENERGY FOR IMPLANTATION IN DONOR SUBSTRATE AND METHOD FOR MANUFACTURING SEMICONDUCTOR TYPE STRUCTURE ON INSULATION
FIELD OF THE INVENTION
The present invention relates to a method of manufacturing a layer transfer structure. This method is more particularly used to fabricate SeOI type structures (acronym for the term "Semiconductor On Insulator" or Semiconductor on Insulator) by a SmartCut ™ type technique.
BACKGROUND OF THE INVENTION
The Smart Cut ™ process allows the transfer of a thin semiconductor layer from a donor substrate to a receiving substrate and implements the following steps; a) Implantation of atomic species in the donor substrate in order to create an embrittlement zone whose depth corresponds to the thickness of the thin layer that it is desired to transfer. b) Contacting the substrates and bonding by molecular adhesion.
Bonding is done over the entire surface of the substrates except at the periphery, because the plates have a chamfer (or "Edge Roll Off" (ERO) according to the English name) and are therefore not in contact on their periphery, as it can be seen in FIG. 1. c) Detachment according to the zone of weakness of the donor substrate, and transfer of the thin layer towards the substrate received.
The substrates are generally in the form of circular plates (also called "wafers" in the language of the trade); for example, 300 mm plates are commonly used.
The ring region is called the peripheral region where the transfer of the thin layer has not occurred. With reference to FIG. 2, which represents in top view four peripheral regions of a SeOI plate, the ring gear CP is delimited on the outer side by the edge 100 of the receiving substrate and on the inside by the edge 200 of the layer transferred. . On the plate of Figure 2, the crown CP is regular, ie the edge of SeOI is regular.
However, in some cases, an irregular crown width (also called "jagged edge" according to the trade vocabulary) on the final product, that is to say the SeOI obtained after detachment. After detachment, the crown may also include small isolated transferred areas.
The crown width is thus made irregular by the local and uncontrolled extension of the transferred area several hundred micrometers to the edge of the receiving substrate.
A situation where an irregular ring is observed is the implementation of activation, for example by plasma, of the surface of at least one of the substrates before bonding by molecular adhesion. This activation significantly enhances the bonding energy. The reinforcement of the bonding energy can also be obtained by cleaning before suitable bonding, for example a sequence of the type 03 / SC1 / SC2 in which the SC1 is produced at a temperature below 50 ° C.
The patent application WO 2009/034113 in the name of the Applicant proposes to overcome this disadvantage by controlling the activation of the surface of the substrate so that the increase of the bonding energy between the donor substrate and the receiving substrate or, in a peripheral region of these substrates, less than the increase in the bonding energy in the central region of said substrates.
However, there are still situations where the "jagged edge" phenomenon is observed, even when the aforementioned control is implemented. These include the cases where the transferred semiconductor layer has a large thickness, that is to say typically greater than or equal to 370 nm, and where the weakening zone is formed by co-implantation of two different species. , usually hydrogen and helium.
However, this unwanted transfer in the ring creates a brittle area in which the transferred semiconductor layer is susceptible to chemical attack by its interface with the receiving substrate (phenomenon called "under etching" according to the English terminology). and delaminate. This may result in particulate contamination of the SeOI structure that renders it non-compliant with product specifications.
One solution to remedy this type of defect would be to remove the zones transferred into the crown by a mechanical or chemical action.
However, the implementation of such recovery operations would be complicated to implement on an industrial scale and would reduce the cost of manufacturing SeOI structures.
BRIEF DESCRIPTION OF THE INVENTION
One of the aims of the invention is therefore to improve the method of manufacturing a layer transfer structure so as to guarantee a regular transferred layer edge, without local extension. To this end, the invention relates to a method for determining a suitable energy for implantation of at least two atomic species in a donor substrate to create a weakening zone defining a semiconductor monocrystalline layer to be transferred on a receiving substrate. including the following steps; (i) forming a dielectric layer on at least one of the donor substrate and the receiving substrate, (ii) co-implantation of said species in the donor substrate with a determined energy to form the weakening zone, (iii) bonding of the donor substrate on the receiving substrate such that said dielectric layer is at the bonding interface, (iv) detaching the donor substrate along the embrittlement zone (31) so as to transfer the semiconductor monocrystalline layer and recovering a remainder of the donor substrate, (v) inspecting the peripheral ring of the remainder of the donor substrate or the peripheral ring of the receiving substrate on which the semiconductor monocrystalline layer has been transferred to step (iv), (vi) if said ring has zones transferred to the receiving substrate, determining that the implantation energy of step (ii) is too high, * (vii) if said uronne does not have transferred areas on the receiving substrate, determining that the implantation energy of step (ii) is suitable.
Advantageously, step (ii) is carried out on a plurality of donor substrates with different respective implantation energies and it is determined from the inspection of the remainder of the donor substrate or the receiving substrate on wherein the monocrystalline semiconductor layer has been transferred obtained for each of said implantation energies, a suitable implantation energy range.
Thus, one can determine the maximum implantation energy in said range of suitable implantation energy and deduce the maximum thickness of the semiconductor monocrystalline layer to be transferred to the receiving substrate.
Another subject of the invention relates to a method of manufacturing a semiconductor-on-insulator type structure by transfer of a semiconductor monocrystalline layer from a donor substrate to a receiving substrate, comprising the following steps: determining a suitable implantation energy by the method as described above, (b) forming a dielectric layer on at least one of the recipient substrate and the donor substrate, (c) co-implantation of atomic species, such as hydrogen and helium, with the implantation energy determined in step (a), to create an embrittlement zone in the donor substrate so as to define a semi-crystalline monocrystalline layer -conductor to be transferred, (d) molecular bonding of the donor substrate to a receiving substrate, said dielectric layer being at the bonding interface, (e) detachment of the donor substrate according to the area of de gilization, so as to transfer the semiconductor monocrystalline layer on the receiving substrate.
According to one embodiment of the invention, the suitable implantation energy determined in step (a) corresponds to a thickness of the layer transferred in step (e) less than the desired thickness for the layer. semiconductor process of the semiconductor-on-insulator structure, said method further comprising, after step (e), a step (f) of epitaxial growth on the transferred layer on the donor substrate until obtaining the desired thickness.
BRIEF DESCRIPTION OF THE DRAWINGS Other features and advantages of the invention will become apparent from the detailed description which follows, with reference to the appended figures in which;
FIG. 1 is a sectional photo of two glued plates showing the chamfers of the plates at the origin of the SeOI ring; FIG. 2 is a top view of the edge of a SeOI plate having a regular ring; FIG. 3 is a sectional view of a structure after bonding a donor substrate to a receiving substrate to manufacture a SeOI; FIG. 4 is a sectional view of the preceding structure after detachment and transfer of a semiconductor monocrystalline layer; - Figure 5 is a sectional view of the structure of Figure 4 after the implementation of an epitaxial recovery on the transferred layer. FIGS. 6A to 6C are inspection images of the peripheral ring of the remainder of a donor substrate for different implantation energies corresponding to different thicknesses of the transferred layer (respectively 350 nm, 420 nm and 600 nm).
DETAILED DESCRIPTION OF EMBODIMENTS OF THE INVENTION
FIG. 3 illustrates the structure obtained after gluing a donor substrate 30 onto a receiving substrate 10.
During the implementation of the Smart Cut ™ process, the donor substrate 30 (and / or the receiving substrate) may for example be covered with a dielectric layer 20, in particular an oxide layer. As is well known to those skilled in the art, the oxide may be deposited or formed by thermal oxidation of the donor substrate.
The donor substrate 30 then undergoes co-implantation of at least two atomic species, such as, for example, hydrogen and helium, the dose and energy of which are adapted so as to obtain a peak of implantation at a depth corresponding to the thickness of the layer of the donor substrate that it is desired to transfer. The zone 31 where the atomic species are implanted is called zone of weakening. Thanks to this co-implantation, the helium atoms contribute to confining the hydrogen atoms, which makes it possible to improve the quality of the subsequent detachment along the embrittlement zone. The implantation of these two species is carried out in a time-shifted manner. Moreover, the implantation energies of the two species (which depend on the weight of the respective species) are not necessarily identical. Those skilled in the art are able to define the dose and energy parameters for the two species depending on the depth of the weakening zone to be formed.
After possible plasma activation of the surface of the donor substrate 30 and / or the receiving substrate 10, the substrates are contacted and bonded by molecular adhesion. Plasma activation has the effect of increasing the bonding energy between the two substrates. This increase in the bonding energy can also be obtained by means of cleaning before bonding type O3 / RCA in which the ICS is carried out at a temperature below 50 ° C. This cleaning is well known to those skilled in the art and will not be described in detail. It is simply recalled that the RCA comprises a series of so-called baths SCI and SC2. ICS is a mixture of H2O, H2O2 and NH4OH. SC2 is a mixture of H2O, H2O2 and HCl. Rinses in H2O are inserted between these baths of SCI and SC2. Cleaning O3 corresponds to a first bath of H20 in which ozone gas is dissolved.
As can be seen in FIG. 3, the plates of the two substrates do not have an edge perpendicular to the surface but have a chamfer or "Edge Roll Off" designated by the arrows C. The substrates 10 and 30 are therefore not not glued to their edge but up to the chamfer.
The donor substrate 30 is then detached along the embrittlement zone 31. For this purpose, detachment can be initiated by means of mechanical forces or a rise in temperature; detachment propagating over the entire surface in the form of a detachment wave. The SeOI structure thus obtained is shown in FIG. 4. Owing to the presence of the chamfers on the edges of the plates, the transferred part of the donor substrate 30 does not normally extend over the entire surface of the receiving substrate 10 but only up to at the limit of a CP peripheral ring.
For a 300 mm plate, the peripheral ring CP typically has a width of 1 mm from the edge of the plate.
The "jagged edge" phenomenon explained in the introduction results in the presence of transferred zones (that is to say oxide 20 and thin layer 32) inside the peripheral ring CP.
The phenomenon of "jagged edge" seems to be due to the fact that the hydrogen and helium implantation energies to create the zone of weakening are too important.
However, such energies may be required to form an embrittlement zone deep enough to be able to transfer a thick enough semiconductor layer.
Thus, the inventors have observed that when the oxide layer is thick (of the order of 0.7 to 3 μm), the surface roughness of the silicon transferred by the implantation and bonding process is greater. Therefore, treatment to smooth the surface of the transferred thin layer and remove implantation defects will lead to significant shrinkage of material, resulting in the need for the deepest possible implantation to transfer a thick enough layer. to obtain the desired thickness after polishing.
Furthermore, the inventors have identified that there is a critical thickness of the layer to be transferred beyond which the fracture wave used for the detachment tends to press the peripheral ring of the donor substrate against that of the receiving substrate - to which it was not bonded initially - which causes a transfer of material from the donor substrate into the peripheral ring of the receiving substrate. This critical thickness depends on the structure in which the detachment is performed, including the thickness of the layer to be transferred. In general, the invention makes it possible to avoid or at least to reduce the "jagged edge" phenomenon by identifying beforehand a range of implantation energy (or at least one implantation energy value). ) for each species not leading to the presence of transferred areas in the peripheral ring of the recipient substrate (this suitable energy being determined by inspecting the peripheral ring of the remainder of the donor substrate after detachment) and using an implantation energy in said range (or less than or equal to the value identified) for transferring a semiconductor monocrystalline layer from the donor substrate to the receiving substrate. Optionally, if the implantation energy used corresponds to a thickness of the transferred layer less than the desired thickness for the thin semiconductor layer of the final SeOI structure, an epitaxy is applied on the transferred layer until obtaining the desired thickness. The invention therefore makes it possible, in a first step, to determine, for a particular SeOI structure to be manufactured, a suitable implantation energy for the two species to be implanted to form the zone of weakening.
This determination method involves the production of several test structures SeOI, each corresponding to different co-implantation energies, in order to determine a window of the implantation process making it possible to limit or even avoid the formation of the jagged edge. ".
More specifically, the manufacture of SeOI test structures comprises the following steps (see FIG. (i) forming a dielectric layer (typically an oxide) on at least one of the donor substrate 30 and the receiving substrate 10, (ii) co-implantation of the species into the donor substrate 30 with a determined energy to form the embrittlement zone 31, (iii) bonding of the donor substrate 30 to the receiving substrate 10 so that said dielectric layer is at the bonding interface, (iv) detachment of the donor substrate 30 along the embrittlement zone ( 31) so as to transfer the semiconductor monocrystalline layer 32 and recover a remainder 34 of the donor substrate.
The remainder 34 of the donor substrate is used to determine whether or not the co-implantation conditions of step (ii) have led to a "jagged edge" phenomenon. For this purpose, the peripheral ring CP of the remainder 34 of the donor substrate is inspected by a device called Edgescan ™, which makes it possible to observe the defects present at the periphery of a substrate. Such equipment is widely used on SeOI structure production lines and will not be described in detail here.
This inspection makes it possible to reach the following conclusions: - if the ring of the remainder of the donor substrate has areas which have been transferred onto the receiving substrate (revealing the "jagged edge"), the implantation energy of the step (ii ) is too high; if said ring does not have zones transferred onto the receiving substrate (meaning that the "jagged edge" has not occurred), the implantation energy of step (II) is suitable.
Optionally, this inspection could be carried out on the SeOI structure, which corresponds to the negative imprint of the remainder of the donor substrate. However, the inspection of the remainder has the advantage of being able to be performed in parallel with the process of manufacturing the SeOI structures which continues.
By performing this approach for different implantation energies, a range of implantation energy is thus determined which makes it possible to avoid the formation of the "jagged edge".
Thus, for the subsequent manufacture of SeOI structures, use will be made of implantation energy located in said range.
The manufacture of these SeOI structures is carried out according to the Smart Cut ™ method and provides a SeOI structure as shown in Figure 4 substantially devoid of "jagged edge". The remainder of the donor substrate can be removed or recycled for another use.
As seen in Figure 4, the thickness of the layer 32 transferred to the receiving substrate is denoted E1.
In the case where it is desired for the thin layer of the SeOI structure to have a thickness E2 greater than E1, this additional thickness is obtained by carrying out an epitaxial step on the transferred layer 32 until obtaining the desired thickness. desired thickness E2 (final layer 33 shown in FIG. 5).
The proper implantation energy range may vary depending on the thickness of the buried oxide layer. Therefore, it will be possible to implement the method of determination described above for SeOI structures having different characteristics (in terms of materials, thickness of the oxide layer, etc.).
Although helium and hydrogen are generally not implanted with the same energy, the energy of helium implantation is defined according to the energy of implantation of hydrogen: the energy of implantation of the hydrogen is determined to obtain a determined depth of the zone of weakening, then the energy of implantation of the helium is determined so that the peak of implantation of the helium is in the vicinity of the peak of implantation hydrogen. Therefore, in the present invention, it is sufficient to determine the proper hydrogen implantation energy, and one skilled in the art is then able to determine the energy of implantation of the helium to be used.
FIGS. 6A to 6C are views of an Edgescan ™ inspection of the peripheral ring CP of the remainder of the silicon donor substrate of an SOI structure with an oxide layer 1 μm thick for different implantation energies of hydrogen between 32 keV and 68 keV. Figure 6A corresponds to an implantation depth of 350 nm, Figure 6B to a depth of 420 nm and Figure 6C to a depth of 600 nm. Although the donor substrate is circular, the image obtained by Edgescan ™ represents the contour of the substrate in the form of a straight line.
In Figure 6A, the peripheral ring CP (which corresponds to a thickness of silicon not transferred to the receiving substrate), the limit of which relative to the central portion of the substrate is designated by the thick arrow, is substantially regular. Note that this ring has a bubbled appearance that is due to implantation.
In Figure 6B, it is observed that the peripheral ring is less regular. In particular, the zones designated by the thick arrows correspond to a transfer of silicon from the donor substrate to the receiving substrate.
In FIG. 6C, it is observed that with the exception of a few zones designated by the thick arrows, the silicon of the peripheral ring has been transferred onto the receiving substrate (the appearance of the peripheral ring being similar to that of the part central substrate). This seems to be explained by the fact that the layer to be transferred was rather rigid and that the detachment was violent enough that the donor substrate, which was initially not bonded to the donor substrate in the region of the chamfer, was flattened. on its edge against the donor substrate, which has led to a transfer of almost all of the donor substrate on the receiving substrate.
It is deduced from these figures that the implantation energies leading to implantation depths of 420 and 600 nm induce a "jagged edge" phenomenon and are therefore too high. On the other hand, implantation energy leading to an implantation depth of 350 nm is suitable.
Therefore, for the manufacture of SOI having an oxide layer of 1 μm thick, it will advantageously carry out co-implantation of hydrogen and helium to reach an implantation depth of at most 370 nm. Optionally, if the silicon layer of the SOI must have a thickness greater than the thickness of the transferred layer, the required thickness will be obtained by means of an epitaxy.
权利要求:
Claims (5)
[1" id="c-fr-0001]
A method of determining a suitable implantation energy of at least two atomic species in a donor substrate (30) to create an embrittlement zone (31) defining a single-crystal monocrystalline layer (32) to be transferred on a receiving substrate (10), comprising the steps of: (i) forming a dielectric layer on at least one of the donor substrate (30) and the receiving substrate (10), (ii) co-implantation of said species into the a donor substrate (30) with a determined energy to form the weakening zone (31), (iii) bonding the donor substrate (30) to the receiving substrate (10) so that said dielectric layer is at the bonding interface (iv) detaching the donor substrate (30) along the embrittlement zone (31) so as to transfer the semiconductor monocrystalline layer (32) and recovering a remainder (34) from the donor substrate, (v) inspecting the the peripheral ring of the re liquat (34) of the donor substrate or of the receiving substrate (10) on which the semiconductor monocrystalline layer (32) has been transferred to step (iv), (vi) if said ring has transferred areas on the receiving substrate determining that the implantation energy of step (ii) is too high, (vii) if said ring does not have zones transferred to the receiving substrate, determining that the implantation energy of step (ii) is suitable.
[2" id="c-fr-0002]
2. Method according to claim 1, wherein step (ii) is carried out on several donor substrates with different respective implantation energies and it is determined from the inspection of the remainder (34) of the donor substrate or receiving substrate (10) on which the monocrystalline semiconductor layer (32) has been transferred obtained for each of said implantation energies, a suitable implantation energy range.
[3" id="c-fr-0003]
The method according to claim 2, wherein the maximum implantation energy is determined in said range of suitable implantation energy and the maximum thickness of the monocrystalline semiconductor semiconductor layer (32) is deduced therefrom. transfer to the receiving substrate.
[4" id="c-fr-0004]
A method of manufacturing a semiconductor-on-insulator-type structure by transfer of a semiconductor monocrystalline layer from a donor substrate (30) to a receiving substrate (10), comprising the steps of: determining a suitable implantation energy by the method according to one of claims 1 to 3, (b) forming a dielectric layer on at least one of the receiving substrate (10) and the donor substrate (30) (c) co-implantation of atomic species, such as hydrogen and helium, with the implantation energy determined in step (a), to create an embrittlement zone (31) in the donor substrate (30) to define a semiconductor monocrystalline layer (32) to be transferred, (d) molecular bonding of the donor substrate (30) to a receiving substrate (10), said dielectric layer being bonding interface, (e) detachment of the donor substrate (30) ) according to the zone of weakening (31), so as to transfer the layer (32) monocrystalline semiconductor on the receiving substrate.
[5" id="c-fr-0005]
5. Method according to claim 4, wherein the appropriate implantation energy determined in step (a) corresponds to a thickness (El) of the layer transferred in step (e) less than the thickness (E2 ) desired for the semiconductor monocrystalline layer (33) of the semiconductor-on-insulator structure, said method further comprising, after step (e), a step (f) of epitaxy on the transferred layer (32) on the donor substrate (10) until the desired thickness (E2) is obtained.
类似技术:
公开号 | 公开日 | 专利标题
WO2017149253A1|2017-09-08|Method for determining a suitable energy for implantation in a donor substrate and process for fabricating a semiconductor-on-insulator structure
EP1879220A2|2008-01-16|Direct water-repellent gluing method of two substrates used in electronics, optics or optoelectronics
EP1208593A1|2002-05-29|Method for treating substrates for microelectronics and substrates obtained by said method
FR2867310A1|2005-09-09|TECHNIQUE FOR IMPROVING THE QUALITY OF A THIN LAYER TAKEN
WO2002037556A1|2002-05-10|Method for making a stacked structure comprising a thin film adhering to a target substrate
FR2874455A1|2006-02-24|HEAT TREATMENT BEFORE BONDING TWO PLATES
FR2892228A1|2007-04-20|METHOD FOR RECYCLING AN EPITAXY DONOR PLATE
FR2889887A1|2007-02-23|METHOD FOR DEFERING A THIN LAYER ON A SUPPORT
EP2302671A1|2011-03-30|Bonding process andlayer transfer method
FR2920912A1|2009-03-13|METHOD FOR MANUFACTURING A LAYER TRANSFER STRUCTURE
EP1777735A2|2007-04-25|Recycling process of an epitaxial donor wafer
FR2938118A1|2010-05-07|METHOD FOR MANUFACTURING A STACK OF THIN SEMICONDUCTOR LAYERS
EP2302666B1|2017-11-01|Process of planarisation by ultrasounds of a substrate whose surface was released by fracture of a weakened buried layer
FR3051596A1|2017-11-24|METHOD FOR MANUFACTURING A CONDUCTIVE SEMICONDUCTOR TYPE SUBSTRATE ON INSULATION
WO2014154978A1|2014-10-02|Process for manufacturing a composite structure
FR2842646A1|2004-01-23|Increasing area of useful layer of material transferred to support substrate when making composite substrate for optics by bonding substrates such that inner outline of chamfer of substrate is inscribed within outline of other substrate
EP3721467B1|2021-12-29|Method for preparing the remainder of a donor substrate, substrate produced by said method, and use of such a substrate
FR3093859A1|2020-09-18|Method of transferring a useful layer onto a support substrate
FR3093860A1|2020-09-18|Method of transferring a useful layer onto a support substrate
FR2915624A1|2008-10-31|Semiconductor material substrates e.g. donor substrate, splicing method, involves applying heat treatment of insulation degassing to substrates or between substrates if substrates support two isolating layers
FR3093858A1|2020-09-18|Method of transferring a useful layer onto a support substrate
FR3059149A1|2018-05-25|PROCESS FOR PRODUCING A THIN FILM BASED ON INP OR GAAS
WO2021009459A1|2021-01-21|Process for hydrophilically bonding substrates
FR3064398A1|2018-09-28|SEMICONDUCTOR TYPE STRUCTURE ON INSULATION, ESPECIALLY FOR A FRONT-SIDE TYPE IMAGE SENSOR, AND METHOD FOR MANUFACTURING SUCH STRUCTURE
EP1839332A2|2007-10-03|Formation and treatment of a sige structure
同族专利:
公开号 | 公开日
JP2019511112A|2019-04-18|
JP6965260B2|2021-11-10|
US20190074215A1|2019-03-07|
CN108701627A|2018-10-23|
FR3048548B1|2018-03-02|
WO2017149253A1|2017-09-08|
US10777447B2|2020-09-15|
TW201735124A|2017-10-01|
TWI724114B|2021-04-11|
SG11201807344RA|2018-09-27|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
EP1777735A2|2005-10-18|2007-04-25|S.O.I.Tec Silicon on Insulator Technologies|Recycling process of an epitaxial donor wafer|
US20070148917A1|2005-12-22|2007-06-28|Sumco Corporation|Process for Regeneration of a Layer Transferred Wafer and Regenerated Layer Transferred Wafer|
US20120199956A1|2011-02-08|2012-08-09|Monique Lecomte|Method for recycling a source substrate|
FR2880988B1|2005-01-19|2007-03-30|Soitec Silicon On Insulator|TREATMENT OF A LAYER IN SI1-yGEy TAKEN|
US7575988B2|2006-07-11|2009-08-18|S.O.I.Tec Silicon On Insulator Technologies|Method of fabricating a hybrid substrate|
FR2920912B1|2007-09-12|2010-08-27|S O I Tec Silicon On Insulator Tech|METHOD FOR MANUFACTURING A LAYER TRANSFER STRUCTURE|
FR2926672B1|2008-01-21|2010-03-26|Soitec Silicon On Insulator|PROCESS FOR MANUFACTURING LAYERS OF EPITAXY MATERIAL|US10224233B2|2014-11-18|2019-03-05|Globalwafers Co., Ltd.|High resistivity silicon-on-insulator substrate comprising a charge trapping layer formed by He-N2 co-implantation|
CN108780776A|2015-11-20|2018-11-09|环球晶圆股份有限公司|Make the manufacturing method that semiconductor surface is smooth|
FR3063176A1|2017-02-17|2018-08-24|Soitec|MASKING A ZONE AT THE EDGE OF A DONOR SUBSTRATE DURING AN ION IMPLANTATION STEP|
US10818540B2|2018-06-08|2020-10-27|Globalwafers Co., Ltd.|Method for transfer of a thin layer of silicon|
法律状态:
2017-02-22| PLFP| Fee payment|Year of fee payment: 2 |
2017-09-08| PLSC| Publication of the preliminary search report|Effective date: 20170908 |
2018-02-20| PLFP| Fee payment|Year of fee payment: 3 |
2020-02-20| PLFP| Fee payment|Year of fee payment: 5 |
2021-02-25| PLFP| Fee payment|Year of fee payment: 6 |
2022-02-21| PLFP| Fee payment|Year of fee payment: 7 |
优先权:
申请号 | 申请日 | 专利标题
FR1651747A|FR3048548B1|2016-03-02|2016-03-02|METHOD FOR DETERMINING APPROPRIATE ENERGY FOR IMPLANTATION IN DONOR SUBSTRATE AND METHOD FOR MANUFACTURING SEMICONDUCTOR TYPE STRUCTURE ON INSULATION|
FR1651747|2016-03-02|FR1651747A| FR3048548B1|2016-03-02|2016-03-02|METHOD FOR DETERMINING APPROPRIATE ENERGY FOR IMPLANTATION IN DONOR SUBSTRATE AND METHOD FOR MANUFACTURING SEMICONDUCTOR TYPE STRUCTURE ON INSULATION|
CN201780014686.1A| CN108701627A|2016-03-02|2017-03-02|Method for determining the suitable Implantation Energy in donor substrate and the technique for manufacturing semiconductor-on-insulator structure|
TW106106821A| TWI724114B|2016-03-02|2017-03-02|Method for determining a suitable implanting energy in a donor substrate and process for fabricating a structure of semiconductor-on-insulator type|
SG11201807344RA| SG11201807344RA|2016-03-02|2017-03-02|Method for determining a suitable implanting energy in a donor substrate and process for fabricating a structure of semiconductor–on–insulator type|
JP2018545988A| JP6965260B2|2016-03-02|2017-03-02|How to determine the appropriate energy for injection into the donor substrate, and how to assemble the Semiconductor-on-insulator structure.|
PCT/FR2017/050471| WO2017149253A1|2016-03-02|2017-03-02|Method for determining a suitable energy for implantation in a donor substrate and process for fabricating a semiconductor-on-insulator structure|
US16/081,816| US10777447B2|2016-03-02|2017-03-02|Method for determining a suitable implanting energy in a donor substrate and process for fabricating a structure of semiconductor-on-insulator type|
[返回顶部]