专利摘要:
The aim of the invention is to provide an inner paste coating in the form of an at least two-component system comprising component A and component B, wherein component A comprises an organic binder and a mineral binder comprising an aluminous cement and / or a Calcium sulfo-aluminous cement, a setting blocker, mineral fillers, a rheological additive, a setting regulator / accelerator, optionally a base, the concentrations of the setting regulator / accelerator and the base in A being such that the pH of the Part A is below the set point of Part A; and component B has a base present in Part B at a concentration to reach a final pH value greater than or equal to the setting threshold of Part A. The application method, as well as the mixing / spraying device for the implementation of said method are also part of the invention.
公开号:FR3044660A1
申请号:FR1561884
申请日:2015-12-04
公开日:2017-06-09
发明作者:Staffan Berglind;Audrey Maratrat;Thierry Jeannette;Frederic Savall
申请人:Cromology;
IPC主号:
专利说明:

INTERNAL PATE COATING, METHOD OF APPLICATION AND DEVICE FOR MIXING AND PROJECTING THE COATING
Technical area
The technical field of the invention is that of interior coating paste for the building.
More specifically, the present invention relates to an inner coating paste, comprising a two-component system to be mixed at the time of use, based on organic binder and calcium aluminate. It also relates to the method of application of said coating, and its mixing / projection device.
Technological background
Interior coatings for the building cover the following areas of application: paint coatings for the preparation of substrates (according to NF T 30-608 and EN16566), jointing plasterboards (according to EN 13963) masonry coatings for plasterboard inside (EN 15824)
Traditionally, interior coatings exist in the form of powder, mainly based on mineral and / or hydraulic binder, and in the form of ready-to-use paste (mainly based on organic binder). Each of these two forms has advantages and disadvantages for the user. On the one hand, the products in the form of powder are stored in powder form in bags, before being mixed with water during implementation on building sites. Powder coatings can be applied in thick layers with low drying shrinkage and their waiting time between two layers ("repetition time") and drying are relatively short. On the other hand, their manipulation requires the use of mixing tools, and scrupulously respect the determined ratios of powder and water, otherwise obtaining a product that does not have the desired properties for application on the support. However, the respect of the ratios of mixing powder / water is not easiest on the building sites. The use of these powder products also has the disadvantage of producing large dust emissions that can be particularly troublesome for the user. On the other hand, products in the form of organic binder paste, despite their convenience because of their "ready-to-use" nature, have a number of disadvantages compared to plaster-based powder coatings. or with respect to cement-based mortars, which limit their use, namely: drying time: under adverse application conditions (cold, humidity, lack of ventilation) drying by evaporation is longer than hydration drying (setting) of mineral binder products. sensitivity to water: if a coating based solely on low-dose polymeric binders (usually 1.5% to 3% solids equivalent for a standard coating) is soggy after drying with a water supply, then The coating is weakened and adhesion and / or take-off problems may occur. drying shrinkage: for thick-fillings, the shrinkage of paste coatings is too strong (usually 10 to 20% by volume) limiting their practical use to thicknesses of less than 5mm per layer for the best, and practical at less than 2 mm. In addition, for such large thicknesses, the drying time is very long, while a plaster based coating reduces the shrinkage to generally less than 3% for thicknesses up to 25 mm.
In an attempt to overcome these disadvantages, coatings having two-component systems have been developed. In this case, the mixture of the two components initiating the curing reaction of the dough, is made just before the implementation on the support, thereby reducing the drying time, even in adverse weather conditions. Another advantage of this type of system is to be able to combine the advantages of the two types of inorganic and organic binder in order to obtain a coating with improved performances.
Application EP0496682A1 describes a coating for filling joints between two plasterboards, which is in the form of two components which are kept separately, the first component containing plaster in the powdered state, and a second liquid or pasty component consisting of a copolymer polymer of vinyl acetate and ethylene in an aqueous medium acting as the main binder of the joint. This coating advantageously has a relatively low plaster content of less than 30%, as well as a good mechanical strength to ensure durability and resistance to impact, as well as fast curing kinetics. It has the disadvantage of requiring the user to handle a powdery product.
Application for a utility certificate FR2763937 describes a two-component aluminous cement system for buildings, applicable to the field of building chemistry, and in particular to gluing or sealing materials. Compound A is in the form of aqueous paste and consists of a polymer resin and an aluminous cement suspended in water, the hydration of which is momentarily stopped by a boric acid-based retarder, as well as an organic dispersant, a thickening agent and mineral fillers. The compound B for initiating the hardening of the cement is also in the form of an aqueous paste, and is composed of a mixture of hydrated lime and a sodium salt. When compound A and compound B are mixed, the pH of the mixture increases rapidly, which initiates the curing. The proportions between compound A and compound B are determined by the desired time between mixing and beginning of hardening.
Patents EP0241230 and EP0113593 also disclose two-component systems comprising on the one hand a base component comprising cement and a retarder, and on the other hand a catalyst consisting of lime and lithium salt, making it possible to obtain setting less than 5 minutes and high mechanical strength.
However, the two-component systems mentioned above are perfectible, because of the toxicity of some of their components vis-à-vis the environment, and their corrosivity which confers a dangerous nature to their handling.
There is therefore a real need for users to have an inner coating paste having the advantages of a two-component system, especially in terms of storage stability, ease of application, and improved mechanical properties after application and curing, while being non-toxic and / or non-corrosive to the environment and / or the user.
Technical problem - Objectives of the invention
In this context, the technical problem at the source of the present invention is to satisfy at least one of the following objectives: - to provide a two-component system in the form of a ready-to-use paste coating stable at storage, - provide a coating paste applicable without handling corrosive substances and / or irritating to the user, - provide a paste coating whose application is little dependent on external working conditions (temperature, hygrometry and ventilation of sites) - to provide a paste coating with the possibility of calibrating an appropriate setting time, - to provide a masonry coating that can be used in full or on the singular points allowing to achieve an airtightness according to the most stringent standards (RT2012 - to provide a coating that can be used as a thick filling compound or patching compound, for example concrete walls or ceilings, which when applied feel a withdrawal reduces drying - offer a projection device with a coating paste, easy to use and maintenance, and reliable.
Brief description of the invention
All or part of the above-mentioned objects is achieved by the present invention which, according to the first aspect, relates to an internal paste coating comprising an at least two-component system comprising a component A and a component B, in which: A - component A includes: a. 1. an organic binder; a.2.a mineral binder comprising an aluminous cement and / or a calcium sulfoaluminum cement; a.3.a setting blocker; a.4. mineral charges; at. 5. a rheological additive; a.6. optionally a non-rheological additive; s.7. optionally a setting regulator / accelerator selected from the group consisting of alkaline and / or alkaline earth compounds such as oxides, hydroxides, carbonates, sulphates and mixtures thereof, or more preferably consisting of lithium hydroxide, lithium carbonate and / or lithium sulphate; a.8.a possible basis • different from the setting regulator / accelerator a.7; Able, in combination with the base b1 defined below, to bring the pH of the mixture to a value V, which is, in increasing order preferably between 6 and 9, between 7 and 9, between 7 and 7; and 8; And preferably chosen from nitrogenous bases and tetrapyrophosphate, 2-amino-2-methyl-1-propanol being preferred; the concentrations of a.7 and a.8 in A being such that the pH of Part A is below the set point of Part A; at. 9. and water; B - component B comprises: b. l. a base • identical to or different from the base a.8; • different from the a.7 regulator / accelerator; Able, in combination with the base a.8 defined above, to bring the pH of the mixture to a value V, which is greater than or equal to 9, preferably greater than or equal to 10; And preferably chosen from nitrogenous bases and tetrapyrophosphate, 2-amino-2-methyl-1-propanol being preferred; this setting accelerator b.l being present in part B at a concentration making it possible to reach a final pH value greater than or equal to the setting threshold of part A; b.2. some water; b.3. optionally, a thickening agent, and; b.4. optionally a setting regulator / accelerator, identical or different from the regulator / setting accelerator a.7 possibly present in component A, and selected from the group comprising alkaline and / or alkaline earth compounds such as oxides, hydroxides, carbonates, sulphates and mixtures thereof, or more preferably consisting of lithium hydroxide, lithium carbonate and / or lithium sulphate; with the condition that the coating necessarily comprises a setting regulator / accelerator present in either component A or component B, or both components A and B, preferably in component B.
In order to trigger the setting of the coating according to the invention, the component A is mixed with the component B, which causes the increase of the pH of the medium, thus rendering inoperative the setting blocker.
It is the merit of the inventors to have succeeded in formulating this coating by using a component B which is: - non-irritating - capable of being incorporated in liquid or pasty form and mixed with a paste comprising an organic binder and a mineral binder, without to hinder the thixotropy of the final coating after mixing A and B so that no sag is formed after application on the support, - able to bring the final pH to a value greater than or equal to the setting threshold of the component A. The coating according to the invention has good performance of implementation such as shrinkage drying, adhesion / cohesion, and less sensitivity to soaking. The paste obtained at the end of the mixing of component A with component B also has a suitable consistency of use, is homogeneous, and has a viscosity such that its application is easy, in particular by projection.
Mineral binding components a. 2 and set retarder a. 3 can be introduced into the mixture either in the form of a pre-established mixture in aqueous suspension ("slurry"), or directly and independently of one another. The order of introduction of the various components must be such that it makes it possible to obtain a stable component A in which the setting of the binder is blocked.
According to a second of its aspects, the invention relates to a process for preparing the coating, by separate blends and taking care to avoid, at any moment, the passage of the pH of the mixture leading to component A, above 8, even above 7.5, and even better above 7.
According to a third of its aspects, the invention also relates to a method of application on a support, preferably an interior building surface of the coating according to the invention comprising the steps of: i-mixing component A with the component B, ii application of the coating obtained preferably by projection / spraying and / or float.
According to a fourth of its aspects, the present invention relates to a mixing / projection device for implementing the method according to the invention comprising: a source of supply of component A; a source of supply of component B; a projection lance provided with a projection head, comprising a mixing chamber of the component A and the component B, and connected to the source of supply of component A and to the source of supply of component B; means for conveying component A from its source of supply to the projection lance; means for conveying component B from its source of supply to the projection lance; optionally projection means of the component A-component B mixture, outside the projection head; and optionally a control device for controlling the mixing ratio component A - component B. Definitions
Throughout this presentation, any singular denotes indifferently a singular or a plural.
The definitions given below as examples may be used in the interpretation of this paper.
By "paste coating" is meant that it is e.g. a coating whose rheology is suitable for application on a support by float or projection. For example, the coating may have a consistency of use of 9-14 caliber measured at the Consistor Baronnie, according to EN 14496.
The term "rheological additive" refers in particular to any additive having an impact on the rheological behavior of the composition, in particular its viscosity and its consistency.
Unless otherwise indicated,% given in this specification are percentages by mass.
Detailed description of the invention
Qualitative and quantitative characteristics of the coating composition
According to a preferred embodiment of the invention, the two-component system is characterized by the fact that neither component A nor component B is considered as corrosive and / or irritating according to the classification system of the chemicals in force, and in particular, none of the components A and B are labeled as corrosive SGH05, nor, preferably, SGH07 irritant according to the Globally Harmonized System of Classification and Labeling of Chemicals (abbreviated as "Globally Harmonized System", GHS; Globally Harmonized System of Classification and Labeling of Chemicals, GHS).
Indeed, one of the aims of the invention, as previously mentioned, is to provide a two-component interior coating whose handling can be done without risk to the manipulator, to improve the practicality and comfort of use, especially by allowing a spray application.
Advantageously, the dry mass ratio [(a1): (a.2)] varies from [1: 3] to [1: 0.5] and the dry mass percentage of (a.2) relative to the total mixture is less than or equal to 6%.
The variation of the inorganic binder ratio on organic binder makes it possible to vary in particular the adhesion of the final coating, and other mechanical and / or physical properties.
According to a preferred embodiment, the coating has the following composition, in mass percentage, in increasing order of preference for each constituent:
For component A: a. 1. organic binder .......................................... [0,5 -5.0]; [l, 9-2.5] a.2.round mineral ............................. ................ [1,0-10,0]; [2,4-6,0] a.3.locker ........ ................................ [0.001 - 1]; [0.01 - 0.5] a.4 .organic loads ....................................... [40,0-80,0 ] [55.0-66.0] a.5. rheological additive ...................................... [0,5-7,0]; [1,4-3] a.6. non-rheological additive ................................. [0,4-3,0]; [0.9-1.4] a.8.base .................................... ..................... [0.05-0.30]; [0.15-0.20] a. 9.eau ............................................... ............ [20-50]; [27-29]
For component B: b. 1.base ............................................... ........... [5.0-20.0]; [8.0-12.0] b.2.water .................................... ....................... [80-95]; [88-92] b.3. thickening agent ....................................... ... [0-1,0]; [0,2-0,5] b.4.adjustment regulator / accelerator ......................... [0,01-3] ; [0.3-2]; [0.7-0.9].
The two-component system according to the invention contains a number of ingredients whose role and definition are given below. • Organic binder a. 1
Advantageously, the organic binder has. 1 is selected from the group consisting of or more preferably consisting of: copolymers of vinyl acetate / ethylene, vinyl ester of versatic acid, or styrene / acrylic / acrylic, alkyd resins, and / or mixtures thereof, preferably in emulsion form. S Take Blocker a.3
The role of the setting blocker is to prevent the setting of the inorganic binder in component A by maintaining an acidic pH.
Advantageously, the setting blocker a.3 is chosen from the group comprising- or better still consisting of-: boric acid, tartaric acid, citric acid, salts and / or derivatives thereof, l. metaphosphoric acid, phosphorous acid, phosphoric acid, phosphonic acid and any compounds capable of forming any of these compounds by reaction with water, and / or their mixtures.
These setting blockers have different mechanisms of action, by limiting the solubilization of the mineral binder in water, or by delaying the massive precipitation of the hydrates corresponding to the setting. Their possible combination makes it possible, by combining their complementary mechanisms of action, to obtain a component A that is stable over time. • S Mineral Loads a.4
Advantageously, the inorganic fillers a.4 are chosen from the group comprising- or better still consisting of-: the non-leaching fillers, preferably selected from the subgroup comprising- or more preferably constituted by: calcium carbonate, quartz, silicates, titanium dioxide, dolomite, and mixtures thereof; The lightening fillers, preferably selected from the subgroup comprising or better still consisting of: the co-esters of aluminum silicates, the water-blown expanded perlites, the glass beads, for example of the type marketed under the brand name PORAVER® (low density expanded glass beads) and their mixtures; • and their mixtures. S Rheological Additive a. 5
Advantageously, the rheological additive comprises at least one compound chosen from at least one of the following families: clays, for example, bentones, smectites, atapulgites (Foulon earth or smectites), cellulose ethers, thickeners synthetic (acrylic, polyurethane), xanthan gums, guar gums, cellulose fibers, modified starch derivatives, and polyvinyl alcohol. • S Nonrheological additive a. 6
According to a preferred embodiment, the non-rheological additive comprises at least one compound chosen from at least one of the following families: biocides, defoamers, anti-flash-rusts, dispersants, and waxes. S Accelerator a.7 and b.4 The function of the Accelerator a.7 or b.4 is to be a regulator of the setting speed, once this is triggered by mixing the component A with component B. S Bases a.8 etb.l
The function of the base a.8 in component A is to increase the pH of the mixture to reach a pH around 7-8, so that the thickeners used to have a stable paste with the desired rheological characteristics are in terms of thixotropy, viscosity, mechanical behavior under shear, etc.
The base a.8 and bl which are advantageously non-corrosive (according to the classification system of the chemicals in force), can be advantageously chosen from Tris (hydroxymethyl) aminomethane, 2-amino-2-ethyl-1,3- Propane-Diol, N-butyldiethanolamine, Tetrapotassium pyrophosphate, and 2-amino-2-methyl-1-propanol.
The base used according to the preferred embodiment of the invention is 2-amino-2-methyl-1-propanol (AMP). By using sufficient dilution of AMP in water (for example, dilution of ΓΑΜΡ90 to 12% in water), the substance is considered non-irritating, unlike other commonly used bases such as soda, potassium hydroxide, or slaked lime Ca (OH) 2 to very low concentrations. Thus, the implementation of the products and their handling on site remains an operation without particular risk, and allows in particular application of the product by projection.
Another advantage is that only a small volume is needed to raise the pH sufficiently to trigger the setting of the coating. Thus, the addition of the additive in small amounts allows incorporation without falling viscosity of the coating beyond the limits to keep normal rheological properties once projected on the walls (must not flow, must be able to smoothed with ease), and without the viscosity of the coating would have to be calibrated to too high level making the projection impossible with the targeted materials.
Application characteristics of Γenduit
According to a preferred embodiment, the coating is selected from the group consisting of: paint coatings for the preparation of substrates, plasterboard grouting coatings, or masonry / interior patching plaster.
The purpose of the present invention is to provide a paint coating for the preparation of the supports (according to NF P 30-608 and EN 16566), in particular thick filling fillers or patching compounds, for example concrete walls or ceilings. (EN15824).
The present invention also aims to provide a plaster for grouting gypsum board (according to EN 13963). The advantage of the invention consists in the possibility of modulating the setting time / drying / recoverability by adjusting the amount of lithium sulphate. This possibility is particularly interesting in winter where the use of paste sealant is not done in practice always in optimal conditions (rules of HR <65%, good ventilation, temperature higher than 5 ° C), which induces too long drying times and risks of poor polymerization. More generally, it is an advantage that can be fired on small sites where the organization does not necessarily allow to wait between two coats of plaster.
Finally, the present invention aims to provide a masonry plaster (in full and on singular points), according to EN15824, before insulation / plasterboard doubling to achieve an airtightness of these structures more efficient, to ensure the conformity of buildings against increasingly stringent standards (RT2012), without having to use lime mortars or projected plasters.
Process for the preparation of [[laster
Preparation of components A &amp; B preparation of the coating according to the invention consists essentially • on the one hand, to mix the constituents of component A, ensuring that the instantaneous pH of the partial mixture remains less than or equal to 8, preferably 7 , 5, and more preferably still 7; • on the other hand, to mix the constituents of component B; • and condition separately, in a sealed manner, away from the air, the components A &amp; B.
Advantageously, the order of introduction and the choice of constituents is made in such a way as to maintain the pH as specified. For example, when a very acidic or very basic component is introduced, it is incorporated in diluted form and / or in a progressive manner.
Procédéetdispositlfddppliçc ^
The method according to the invention passes through the mixing of components A & B and the deposition of one or more layers of this mixture on a support, for example a support present inside or outside, preferably inside. buildings such as a wall, a ceiling ... or any other surface to be coated. One of the advantages of the coating according to the invention is to allow the mechanization of its application on a support. In particular, the projection of the mixture A & B can be done using a device according to the invention, which is described below, by way of non-limiting example a preferred embodiment, with reference to attached drawings in which: - Figure 1 shows a schematic overview of the mixing device / projection; FIG. 2 is a detailed view of the projection lance of the device of FIG. 1; FIG. 2A is a partial longitudinal sectional view A-A of FIG. 2 showing the portion of the projection lance disposed upstream of the projection head according to FIG. 2.
The mixing / projection device shown in FIG. 1 comprises: a supply source of component A; a supply source lb of component B; a source 2 of compressed air; a projection lance 3 consisting of the upstream side of a lance body 4 and a projection head 5, comprising a mixing chamber of component A and component B, and connected to the source of component A supply and component B supply source; a duct 6 connecting the source of the supply of compound A to the upstream end of the lance body 4; a duct 7 connecting the component supply source 1 B to the median zone of the lance body 4, via an injector 8; a duct 9 connecting the source 2 of compressed air to the projection head 5, said duct 9 being equipped in this example with valves 10.
The following are also provided without being apparent in FIG. 1: • means for conveying component A from its source 1a to the spear body 4. These means may be constituted by a pump equipping the supply source, which may be for example a tank, and / or the duct 6 connecting the source 1a to the lance body 4; means for conveying component B from its supply source 1b to the projection lance body 4. These means may be constituted by a pump equipping the supply source lb, which may be for example a tank, and / or the conduit 7 connecting the source lb in the middle of the lance body 4; and optionally a control device for controlling the component A-component B mixing ratio, for example by means of calibrated pipe diameters or an automatically controlled flow meter, and to which can be controlled by means routing component A and or the component B tracking means.
The lance body 4 comprises an upstream opening 11 opening on a housing 12, connected by an intermediate channel 13 and then by an annular duct 14, to a downstream opening 15 of the lance body 4. Between this housing 12 and the intermediate channel 13, is disposed a disc 121 pierced with orifices evenly distributed around the periphery of the disc and allowing the passage of the liquid component A.
This lance body 4 also has in its middle part, above the intermediate conduit 13, a connector 16 on which is connected the supply supply line 7 component B. This connector 16 is in communication with the downstream opening of the body lance 4, through a pipe 17. The latter is formed in a hollow rod 171 attach to the lance body 4 with a nut 141 in which is machined the annular conduit 14 for the passage of the component A.
As shown in Figure 2, this downstream opening 15 opens into the projection head 5, inside which is provided a mixing chamber 18, which communicates with a spray nozzle 19. This mixing chamber of the components A &amp; B is also connected by a connector 20, to the compressed air conveyed through the conduit 9 and allowing the projection of the mixture AB, out of the projection head 5, through the nozzle 19, on the support to be coated. The invention will be better understood on reading the examples which follow and which illustrate a preferred formulation of the coating according to the invention, a mode of preparation of this formulation, an evaluation of the properties of use of this coating formulation, as well as an application of this coating formulation using the device described above.
Example 1 AB Two-Component Coating
S Component A Formulation
F Component Formulation B
Ά Component ratio A / Component B
Method of preparation
The product is formulated in the factory with a neutralization of component A at a pH of about 7.5, low enough to ensure storage stability but high enough that the thickeners can act and give the coating a viscosity of level and stability adequate. The addition of the 12% AMP90 solution makes it possible to initiate a setting of the coating under ambient temperature conditions of approximately 23 ° C. in the course of approximately 10 to 15 hours. Technical results S Removal from drying
The measurement of the drying shrinkage is carried out according to the following protocol: - Use a container (eg petri dish) of height <2cm. - Measure the mass of sieved sand at 200 - pm necessary to fill the container and sharpen it. - Fill the container with plaster and sharpen. - Let dry 7 days. - Measure the mass of sand necessary to fill the withdrawal of the coating in its container by pouring the sand on the container and then straightening it.
The ratio of the mass of sand used to fill the shrinkage of the plaster and the mass of sand used to fill the empty container gives a percentage of shrinkage.
The technical results in terms of drying shrinkage are spectacular, from about 12% to about 2% volume shrinkage by the addition of the hydraulic binder in a coating of this type. Adherence / cohesion The adhesion is carried out according to standard NF EN 1542, or ISO 4624.
The product has a similar adhesion (of the order of 1 N / mm2 on concrete in 1mm thickness) to that of a plaster equivalent paste containing no calcium aluminate, but remains in acceptable adhesions with a fixed limit at 0.5 N / mm2 for a coating
to EN16566, at 0.3 N / mm2 for a coating covered by EN 15824 or, for example, a limit of 0.1 N / mm2 for plaster-based plasters covered by EN 13279.
Example 2: Application Using the Application Device Described above shown in Figures 1, 2, 2A.
A low-pressure (nominal 30-40 bar working pressure) or high pressure (low-pressure 80 to 140 bar) operating pump pump, or with a Speeflo-TYREX type airless hydraulic piston pump (nominal working pressure 180 at 220 bar), allows the routing of component A, from source 1a, to the upstream opening 11 of lance body 4 via conduit 6.
Mixture A & B is necessarily in the mixing chamber 18 of the spray head so that the setting of the product can not cement the inside of the pump or pipes if the material is not rinsed thoroughly after use. .
Component B is fed from a conventional supply source lb, such as a traditional pressure pot with pump (maximum 3.5 bar), with improved components to withstand the high pH of component B .
The diameters of the nozzle 19 and the injector 17i are calibrated to give a mixing ratio corresponding to the desired percentage. As an example of setting flows and pressures, one can have: - A compressed air pressure of spray of 3 bars. - A product supply tank B under air pressure with a product pressure at the outlet between 2 and 3 bars. - A product pressure A at the finish in the spray lance in which the mixing with the product B is in a range of 40 to 100 bar, and with an effective flow of 2 to 5 liters / minute.
权利要求:
Claims (13)
[1" id="c-fr-0001]
An inner paste coating comprising an at least two component system comprising component A and component B, wherein: A - component A comprises: a. 1. an organic binder; a.2.a mineral binder comprising an aluminous cement and / or a calcium sulfoaluminum cement; a.3.a setting blocker; at. 4. mineral charges; at. 5. a rheological additive; a.6. optionally a non-rheological additive; s.7. optionally a setting regulator / accelerator selected from the group consisting of alkaline and / or alkaline earth compounds such as oxides, hydroxides, carbonates, sulfates and mixtures thereof, or more preferably consisting of lithium hydroxide, lithium carbonate and / or lithium sulphate; a.8.a possible basis; • different from the a.7 regulator / accelerator; Able, in combination with the base b1 defined below, to bring the pH of the mixture to a value V, which is, in increasing order preferably between 6 and 9, between 7 and 9, between 7 and 7; and 8; And preferably chosen from nitrogenous bases and tetrapyrophosphate, 2-amino-2-methyl-1-propanol being preferred; the concentrations of a.7 and a.8 in A being such that the pH of Part A is below the set point of Part A; at. 9. and water; B - component B comprises: b. l. a base • identical to or different from the base a.8; • different from the a.7 regulator / accelerator; • able, in combination with the base a.8 defined above, to bring the pH of the mixture to a value V, which is greater than or equal to 9, preferably greater than or equal to 10; And preferably chosen from nitrogenous bases and tetrapyrosphate, 2-amino-2-methyl-1-propanol being preferred; this setting accelerator b.l being present in part B at a concentration making it possible to reach a final pH value greater than or equal to the setting threshold of part A; b.2. water, and; b.3. optionally, a thickening agent; b.4. optionally a setting regulator / accelerator, identical or different from the regulator / setting accelerator a.7 possibly present in component A, and selected from the group comprising alkaline and / or alkaline earth compounds such as oxides, hydroxides, carbonates, sulphates and mixtures thereof, or more preferably consisting of lithium hydroxide, lithium carbonate and / or lithium sulphate; with the condition that the coating necessarily comprises a setting regulator / accelerator present in either component A or component B, or both components A and B, preferably in component B.
[2" id="c-fr-0002]
2. Coating according to claim 1, characterized in that neither component A nor component B, are corrosive and / or irritating, and preferably non-labelable corrosive SGH05, nor, preferably, irritating SGH07 according to the general harmonized system of classification and labeling of chemicals (Globally Harmonized System of Classification and Labeling of Chemicals, GHS).
[3" id="c-fr-0003]
Coating according to Claim 1 or 2, characterized in that the dry mass ratio [(a1): (a.2)] varies from [1: 3] to [1: 0.5] and that dry mass percentage of (a.2) relative to the total mixture is less than or equal to 6%.
[4" id="c-fr-0004]
4. Coating according to one of the preceding claims, characterized in that it has the following composition, in percent by weight, in increasing order of preference for each component: For component A: combining organic ..... ........................................... [0.5 -5, 0]; [l, 9-2,5] a.2.round mineral ................................ ................. [1,0-10,0]; [2,4-6,0] a.3.locker ....... .................................. [0.001 - 1]; [0.01 - 0.5] a .4 mineral fillers ....................................... [40,0-80 , 0], [55.0-66.0] a. 5. rheological additive ............................................. [ 0.5-7.0]; [1,4-3] a.6. non-rheological additive ...................................... [0,4-3,0] ; [0.9-1.4] a.8.base .................................... ..................... [0.05-0.30]; [0.15-0.20] a.9.water .................................... ....................... [20-50]; [27-29] For component B: b. 1.base ............................................... ........... [5.0-20.0]; [8.0-12.0] b.2.water .................................... ....................... [80-95]; [88-92] b.3. thickening agent ....................................... ... [0-1,0]; [0,2-0,5] b.4.adjustment regulator / accelerator ......................... [0,01-3] ; [0.3-2]; [0.7-0.9].
[5" id="c-fr-0005]
5. Coating according to at least one of the preceding claims, characterized in that the organic binder is selected from the group comprising- or more preferably constituted by: copolymers of vinyl acetate / ethylene, vinylester of acid versatic, styrene / acrylic / acrylic, alkyd resins and / or mixtures thereof, preferably in emulsion form.
[6" id="c-fr-0006]
6. Coating according to at least one of the preceding claims, characterized in that the setting blocker a.3 is selected from the group comprising- or better still consisting of-: boric acid, tartaric acid, citric acid, salts and / or derivatives thereof, metaphosphoric acid, phosphorous acid, phosphoric acid, phosphonic acid and any compounds capable of forming any of these compounds by reaction with the water, and / or mixtures thereof.
[7" id="c-fr-0007]
7. Coating according to at least one of the preceding claims, characterized in that the inorganic fillers a.4 are chosen from the group comprising- or better still consisting of-: • the non-leaching fillers, preferably selected from the sub- group comprising or more preferably consisting of: calcium carbonate, quartz, silicates, titanium dioxide, dolomite, and mixtures thereof; • Lightening fillers, preferably selected from the subgroup comprising- or better still consisting of: aluminum silicate cenospheres, water-blown expanded perlites, glass beads, and mixtures thereof; • and their mixtures.
[8" id="c-fr-0008]
8. Coating according to at least one of the preceding claims, characterized in that the non-rheological additive comprises at least one compound selected from at least one of the following families: biocides, anti-foams, anti-flashes -rusts, dispersants, and waxes.
[9" id="c-fr-0009]
9. Coating according to one of the preceding claims, characterized in that the rheological additive comprises at least one compound selected from at least one of the following families: clays, cellulose ethers, synthetic thickeners, xanthans, cellulose fibers, modified starch derivatives, and polyvinyl alcohol.
[10" id="c-fr-0010]
Coating according to at least one of the preceding claims, characterized in that the coating is selected from the group consisting of: paint coatings for the preparation of substrates, plasterboard plaster coatings, or plaster coatings. masonry / patching for the interior.
[11" id="c-fr-0011]
11. A method for preparing the coating according to at least one of the preceding claims, characterized in that it consists essentially • on the one hand, to mix the constituents of component A, by ensuring that the instantaneous pH of partial mixture remains less than or equal to 8, preferably 7.5, and more preferably still 7; • on the other hand, to mix the constituents of component B; • and condition separately, in a sealed manner, away from the air, the components A &amp; B.
[12" id="c-fr-0012]
12. A method of applying to a support, preferably an interior building surface of the coating according to at least one of claims 1 to 10 comprising the steps of: i-mixing component A with component B, ii- application of the coating obtained preferably by projection / spraying and / or floatation.
[13" id="c-fr-0013]
13. Mixing device / projection for implementing the method according to claim 11 comprising: a source of supply of component A; a source of supply of component B; a projection lance provided with a projection head, comprising a mixing chamber of the component A and the component B, and connected to the source of supply of component A and to the source of supply of component B; means for conveying component A from its source of supply to the projection lance; means for conveying component B from its source of supply to the projection lance; optionally projection means of the component A-component B mixture, outside the projection head; - And possibly a control device for controlling the mixing ratio component A - component B.
类似技术:
公开号 | 公开日 | 专利标题
FR3044660A1|2017-06-09|INTERNAL PATE COATING, METHOD OF APPLICATION AND DEVICE FOR MIXING AND PROJECTING THE COATING
EP2822911B1|2019-11-20|Dry composition based on a mineral binder, used for preparing a moist formulation for the building industry
EP1562874B1|2015-07-01|Joint coating composition for construction elements and method for producing a structure
EP1578703B1|2007-04-11|Liquid setting accelerator for a composition comprising portland cement
EP2601152B1|2016-09-07|Pulverulent mortar composition having improved adhesion
FR2722189A1|1996-01-12|NEW PROCESS FOR THE PREPARATION OF A HYDRAULIC COMPOSITE
EP1893548A2|2008-03-05|Fast binder compositions for concrete parts and works containing a calcium salt
CA2470542A1|2003-07-24|Foamed fireproofing composition and method
EP3371127A1|2018-09-12|Dry construction composition wet-sprayable by means of a screw pump and containing abinder and a biosourced filler, and preparation and uses of such a composition
WO2012127066A1|2012-09-27|Dry cement composition for preparing a wet coating formulation consisting of non-efflorescent mortar or cement
FR3050203A1|2017-10-20|STRONG ALLOY MORTAR COMPOSITION AND THERMAL INSULATION
EP0886628B1|1999-11-10|Aqueous silica suspensions and use thereof in inorganic binder compositions
EP2714612B1|2019-07-17|Hydraulic binder comprising an accelerator, its application and process for preparation of a construction material
FR2975096A1|2012-11-16|PROCESS FOR CURING PERMEABLE CONCRETE
EP3630699A1|2020-04-08|Inner paste coating, method of application and device for mixing and spraying the coating
EP3066060B1|2018-08-08|Wetting composition taking the form of a powder and its preparation process
EP2531462B1|2016-04-27|Method for spraying foam material, and coating obtained from such a method
WO2017013376A1|2017-01-26|Method for preparing a glycerine-containing lightweight concrete or mortar
LU82392A1|1980-07-31|IMPROVED JOINING CEMENT
WO1999025664A1|1999-05-27|Hydration modifying agent for mortar or concrete with limited shrinkage
EP3392224A1|2018-10-24|Use of an air-entraining agent for reducing the drying time of a layer made of calcium sulphate
CA2251993C|2003-06-03|Binder substance additive for use in construction, and building material containing such an additive
EP1785406A1|2007-05-16|Method for bonding on gypsum screeds
EP0818426A1|1998-01-14|Process for prolonging the long-term protective effect of cement-based composition against the corrosion of included steel and product for enabling this prolongation
CA2188627A1|1997-04-28|Conglomerate anti-settling additive
同族专利:
公开号 | 公开日
FR3044660B1|2018-01-05|
EP3383820B1|2020-02-05|
WO2017093703A1|2017-06-08|
EP3383820A1|2018-10-10|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
US4088804A|1975-09-08|1978-05-09|Cornwell Charles E|Cementitious coatings and method|
US4455171A|1981-12-09|1984-06-19|Societe Anonyme D'explosifs Et De Produits Chimiques|Reactivatable set-inhibited cementitious compositions|
US4814201A|1987-08-31|1989-03-21|Smith William H|Apparatus and method for applying a layer of fiber on a surface|
US4934596A|1989-01-19|1990-06-19|W. R. Grace & Co.-Conn.|Slurry distributor|
FR2763937A3|1997-06-03|1998-12-04|Lafarge Aluminates|Two-component hydraulic sealing and bonding system|
FR2918055A1|2007-06-28|2009-01-02|Kerneos Sa|BICOMPONENT SYSTEM BASED ON ALUMINOUS CEMENT RETARDED WITH INSTANT TRIP|
WO2011083174A1|2010-01-11|2011-07-14|Parexlanko|Insulating silica xerogel plaster|
EP2431341A1|2010-09-21|2012-03-21|Sto Ag|Compound for creating a quick hardening, completely hard-dried coating on a construction substructure and/or construction element|
EP2607330A1|2011-12-19|2013-06-26|Sto Ag|Dampening system comprising a dampening element and a plaster mass to be applied to the dampening element|
WO2014009298A2|2012-07-10|2014-01-16|Sika Technology Ag|Two component cement composition|
FR3014430A1|2013-12-06|2015-06-12|Lhoist Rech & Dev Sa|BINDER COMPOSITION FOR PERFECT MORTARS AND COATINGS|CN108585759A|2018-07-09|2018-09-28|深圳大学|A kind of cement composite material and the preparation method and application thereof, a kind of concrete composite material and preparation method thereof|
EP3456695B1|2017-09-13|2020-11-11|Dow Global Technologies LLC|Waterborne coating composition|
CN108485333A|2018-05-03|2018-09-04|北京浦立特科技有限公司|Cement gel slurries and preparation method thereof with rust anticorrosive construction|
US20210363062A1|2018-06-25|2021-11-25|Basf Se|Two-component system for formation of cohesive bonds or for chemical anchoring|
US11155498B2|2018-09-28|2021-10-26|Paul Sampson|Cementitious composition with high bond strength to both asphalt and cement based materials|
法律状态:
2016-11-29| PLFP| Fee payment|Year of fee payment: 2 |
2017-06-09| PLSC| Publication of the preliminary search report|Effective date: 20170609 |
2017-10-30| PLFP| Fee payment|Year of fee payment: 3 |
2018-10-30| PLFP| Fee payment|Year of fee payment: 4 |
2019-12-27| PLFP| Fee payment|Year of fee payment: 5 |
2020-02-28| TP| Transmission of property|Owner name: INTERNATIONAL COATING PRODUCTS, FR Effective date: 20200121 |
2020-11-30| PLFP| Fee payment|Year of fee payment: 6 |
2021-10-21| PLFP| Fee payment|Year of fee payment: 7 |
优先权:
申请号 | 申请日 | 专利标题
FR1561884|2015-12-04|
FR1561884A|FR3044660B1|2015-12-04|2015-12-04|INTERNAL PATE COATING, METHOD OF APPLICATION AND DEVICE FOR MIXING AND PROJECTING THE COATING|FR1561884A| FR3044660B1|2015-12-04|2015-12-04|INTERNAL PATE COATING, METHOD OF APPLICATION AND DEVICE FOR MIXING AND PROJECTING THE COATING|
EP16819610.3A| EP3383820B1|2015-12-04|2016-12-05|Indoor paste coating comprising a two-component system and application method|
PCT/FR2016/053215| WO2017093703A1|2015-12-04|2016-12-05|Indoor paste coating comprising a two-component system, application method and device for mixing and projecting the coating|
[返回顶部]