专利摘要:
The invention relates to a method for treating lignocellulosic material, preferably wood, comprising the following steps: (1) soaking the material with organic fluid to dissolve at least 40% and at most 85% by weight of lignin material; (2) washing with an organic fluid so as to evacuate the dissolved lignin; (3) filling with a filling compound; and (4) a finish, so as to obtain a composite material formed of a three-dimensional network of converted filler compound incorporated into a cellulose and lignin network. The invention also relates to a composite material structure thus obtained, and any part comprising at least one such structure.
公开号:FR3044577A1
申请号:FR1561953
申请日:2015-12-07
公开日:2017-06-09
发明作者:Timothee Boitouzet
申请人:Timothee Boitouzet;
IPC主号:
专利说明:

The present invention relates to a lignocellulosic material modification treatment, and any modified lignocellulosic material obtained (referred to as "composite") by this treatment. In particular, the invention relates to a method of partial delignification and filling of a structure of lignocellulosic material, and the structure obtained by this method. The lignocellulosic material is preferably wood.
The wood comprises about 50% of carbon atoms, 6% of hydrogen atoms and 40% of oxygen atoms, as well as traces of metal atoms. More specifically, it is composed of 60 to 75% of carbohydrates in the form of cellulose and hemicellulose, as well as 18 to 35% of lignin, the cellulose being constituted in bundles comprising small inclusions of hemicellulose on the walls of these bundles, lignin serving anarchically, thanks to its transverse chemical bond with hemicellulose, transverse connection between these beams and thus support to the structure. Of course, the internal architecture and the microscopic arrangement of the components depends on the type of wood (softwoods, hardwoods ...) and the essence of wood (fir, white pine, white oak, mahogany, linden, ash .. .).
It is known that certain mechanical properties of wood, such as compressive strength and flexural strength, can be improved by impregnating the wood with at least one monomer and / or polymer. Such wood impregnated with a monomer and / or a polymer is commonly referred to as a wood composite.
A known process for producing wood composite involves immersing the wood to be treated in a fluid such as water, in which the monomer and / or the polymer is dissolved and pressurized. fluid, so as to incorporate the monomer and / or the polymer into the wood. However, such a process is long and requires the use of a high pressure so as to impregnate the wood in depth.
It has therefore been sought to improve this process, for example by using partial vacuum. However, no satisfactory solution has emerged, since all the techniques thus envisaged are penalized by their long duration, mainly because of the difficulty of impregnating the pores of the wood in depth.
It is also known to impregnate the wood with methyl methacrylate (MMA) and then to polymerize the monomer thus impregnated. The polymerization can for example be carried out using high energy radiation such as laser beams or gamma rays. This method is slow, and the use of high energy radiation is particularly expensive. On the other hand, it has been proposed in WO 90/02612 to impregnate wood with a monomer in acidic or basic (alkaline) medium by using supercritical fluid (in the state). This supercritical fluid facilitates the impregnation of the monomer or polymer in the porous material.
A first embodiment proposed in WO 90/02612 comprises the impregnation of the wood with an alkaline or acidic medium in the presence of a first fluid maintained under supercritical conditions, the digestion of the wood impregnated with this medium in the presence of a second fluid maintained under supercritical conditions, so as to extract extractable substances and lignin from wood, which leads to obtaining substantially discrete fibers, which are separated from the supercritical fluid and extractables. The wood thus obtained is recovered and converted into paper. This first embodiment is only reserved for chips ("chips") of wood, since it appears that a very important part, if not all, of the lignin is extracted from the wood, which leads to the destruction of the architecture internal wood. Thus, in the examples of WO 90/02612, these chips are reduced to the pulp state once the extractable substances and the lignin are extracted. The pulp thus obtained, in the form of discrete fibers agglomerated in paste, makes it possible to produce wood panels (agglomerated type) of superior quality in terms of mechanical properties compared with the state of the art.
A second embodiment proposed in WO 90/02612 comprises the treatment of a material containing cellulose with a first fluid in the supercritical state, so as to extract the extractable substances (but not the lignin) from the material comprising the cellulose; separating the supercritical solvent containing the substances extractable from the material, so as to obtain a material comprising fewer extractable substances; contacting the material containing the cellulose and less extractable substances with a second supercritical fluid comprising a polymerizable monomer, under conditions sufficient to allow the impregnation of the monomer into the material; the precipitation of the monomer inside the cellulose; and polymerizing the monomer precipitated in situ, so as to produce a material containing the cellulose. This material has improved properties.
This second embodiment is reserved for pieces of wood of a certain size. Thus, in the examples, large block or logs are treated with either MMA or styrene. However, the use of a supercritical fluid is particularly complicated to implement, especially at the industrial level. Therefore, the solutions proposed in this document do not solve the problems of the state of the art.
More recently, the document WO 2010/089604 has described obtaining pieces of lignocellulosic material produced by impregnating the material with a formulation based on acetic anhydride at acidic pH, and then impregnating the material with a product-based formulation. aqueous organic, followed by pressurization so as to impregnate the two solutions in the material, and then heating so as to crosslink the organic material present in the thus-impregnated cellulosic material. This makes it possible to manufacture a piece of hardened composite Ionic-cellulosic material. However, the filling of the piece of material with the organic product can only be partial or even superficial, which implies that the treatment of a relatively thick piece can not give improved mechanical strength properties.
It has also been described the production of transparent "paper" sheets less than 100 μm thick (Advanced Materials, 2009, 21, 1595-1598, "Optically transparent nanofiber paper", Nogi et al., 2009), in particular by the use of a monomeric compound of acrylic resin (tricyclodecane dimethyl dimethacrylate - TCDDMA-). The production process comprises a total delignification, which leads to obtaining discrete fibers. These fibers are then treated with the resin before being compressed and then crosslinked.
Consequently, to date, the known methods of impregnating wood, or any other lignocellulosic material, to make it a more resistant material, are complicated methods to implement, relatively expensive, and whose implementation The work is much too slow to realistically envisage an industrial production of a composite material of wood.
It remains therefore to this day the need to have a method of treating a structure of lignocellulosic material, preferably wood, so as to obtain a structure retaining the architecture of the wood, and made of a material with improved mechanical properties, particularly in terms of flexural strength and compressive strength, with respect to the lignocellulosic material before treatment. By "lignocellulosic material treatment" is meant here treatment of the material constituting this material.
One of the first objects of the invention is to overcome the aforementioned drawbacks of the methods of the state of the art, and in particular to provide a lignocellulosic material processing method that is simple to implement, which makes it possible to obtain a material retaining the architecture of wood and having improved mechanical, chemical and / or optical properties. The invention thus provides, in a first aspect, a method for treating a structure of lignocellulosic material, the lignocellulosic material preferably being wood, said process comprising the following steps: (1) at least a step of soaking the lignocellulosic material structure with an organic fluid to dissolve at least 40% and at most 85% wt% of the lignin present in the material; (2) at least one step of washing the structure resulting from step (1) by at least one organic fluid so as to evacuate the dissolved lignin resulting from the soaking step (1), so as to produce a structure partially delignified; (3) at least one step of filling the partially delignified structure resulting from the washing step (2) with at least one filling compound, so as to produce a partially delignified filled structure; and (4) at least one step of finishing the partially delignified filled structure resulting from the filling step, (3) so as to obtain a composite material structure formed of a three-dimensional network of converted filling compound incorporated into a cellulose and lignin network.
The transformed filling compound is the compound obtained at the end of the finishing step (4). This finishing step (4) is generally a step of fixing the filling compound, preferably by polymerization and / or crosslinking of the filling compound or compounds, typically when the filling compound comprises at least one monomer. This polymerization or crosslinking is carried out in such a way that fibers of the lignocellulosic starting material are also bonded to the transformed filling compound.
The method for treating a lignocellulosic material structure according to the invention comprises the novel and innovative combination of a partial delignification of the structure followed by a filling by a compound which is stabilized within the structure thus delignified. This combination advantageously makes it possible to obtain a composite material that retains the structure of the material and that has mechanical, chemical and / or optical properties, notably improved with respect to the material before treatment. Without wishing to be bound by any theory, the applicant believes that this is due to the fact that the composite material has molecular bonds between the fibers of the lignocellulosic material stronger than those which exist in the material in the natural state, in particular by intermediate of the transformed filling compound. Thus, the composite material advantageously combines the properties of the wood (lignocellulosic fibers) with those of the transformed filling compound (generally polymeric matrix), by densifying the structure of the composite material in which the transformed filling compound plays the role of continuous binding with respect to the lignin which binds the cell beams punctually anarchically, and adding points of contact between the lignocellulosic fibers together through the transformed filling compound. In general, the transformed filling compound is a polymeric structure, crosslinked or not, which may be locally bonded, by chemical bonding, to said fibers. The Applicant believes that these improved properties can also come from a better organization (improved compactness) and an increase in the crystallinity of the lignocellulosic structure compared to that of the lignocellulosic structure of natural or native wood (in which lignin is amorphous). Thus, in the end, the composite material is formed of a network of lignocellulosic material much denser, and therefore of much greater strength, than the network of lignocellulosic material in the natural state. It is thus possible to qualify the composite material as "hardened". This explains the great qualities of the composite material, and its improved mechanical, chemical and / or optical properties compared to the material before treatment.
By "A and / or B" is meant, according to the invention, A, or B, or A and B.
In a particularly preferred manner, the lignocellulosic material is wood. Virtually all species or families of wood whose lignin content is between 15 and 35%, preferably between 18 and 32%, even more preferably between 20 and 30%, by weight, can be treated by the process according to the invention, either noble wood type oak or ash, or more conventional wood used in the field of furniture or in the field of building (construction). Softwood such as fir, pine, Douglas-fir or hardwood such as linden, poplar, black locust, alder or willow may be mentioned. More generally, softwood is selected from the group consisting of Scots pine, pine, spruce, yew, larch, fir, arole, Douglas fir, araucaria, juniper , cedar, redwood, cedar and cypress, and hardwood is selected from the group consisting of alder, birch, balsa, beech, ash, eucalyptus, cottonwood, rubber, poplar, willow, black locust, oak, mahogany, linden, chestnut, maple, chestnut, elm, hazel, walnut, orange blossom. Osages and the plane tree, it being understood that each family thus mentioned can include many species. For example, the pine family covers more than a hundred species.
The wood can be freshly cut wood, after possible storage of a shorter or longer duration (a few days to a few years), or old wood, that is to say having already been used, for example timber. . Thus, the method according to the invention advantageously allows upgrading by recycling of timber.
But the lignocellulosic material can also be any material formed of a three-dimensional network of cellulose and lignin, such as for example straw, natural textiles (such as flax or hemp), all forest biomass, pulp high efficiency, paper, cardboard, and cotton, if indeed this material is in the form of a structure having a certain mechanical strength and a micro-architecture suitable for being upgraded by a filling compound which partially replaces the lignin.
By "lignocellulosic material structure" is meant according to the invention a three-dimensional object made of lignocellulosic material, and having a certain volume of at least about 2 cm3. Thus, preferably, the lignocellulosic material structure comprises at least one dimension of at least 5 mm and at most 40 cm. When the lignocellulosic material is wood, the structure may be typically a woodcut (cross section, longitudinal section, radial section) for example of thickness 5-7 mm or even 15 mm.
More specifically, the lignocellulosic material structure may be a finishing element, a finishing element or an element of first work.
By "finishing element" is meant according to the invention a three-dimensional object one of whose dimensions, generally the thickness, is much smaller than the other two dimensions and typically at least about 0.5 mm, of preferably at least about 1 mm, even more preferably at least about 2 mm and even more preferably at least about 5 mm. This object is generally selected from the group consisting of wood sheets, inlays, coatings, platelets, plates and veneers, preferably platelets and plates. This corresponds substantially to the term "veneer" in English, preferably "thick veneer". By "finishing element" is meant according to the invention a three-dimensional object one of the dimensions, generally the thickness, is much smaller than the other two dimensions and typically at least about 1 cm, preferably at least 1.5 cm, more preferably at least about 2 cm. This object corresponds typically to the second work in the building, that is to say that it is chosen in the group formed by cladding, cleats, joists, skirting boards, parquet floors, partitions, panels, roof covers and joinery. This corresponds substantially to the term "timber" in English.
According to the invention, the term "element of first work" means a three-dimensional object which is typically a construction element, and whose smallest of the three dimensions is typically at least about 10 cm. This object corresponds to the first work (or structural work) in the building, that is to say that it is chosen from the group formed by columns, beams, lattice structures and frames. This corresponds substantially to the term "lumber" in English.
By "building element" is meant according to the invention an element of the technical field of the building, that is to say a building element, either a finishing element, a second work element or a primary work element .
By "fluid" is meant according to the invention liquid or gas. By "organic" is meant according to the invention containing mainly carbon, hydrogen with oxygen, and nitrogen.
By "dipping" is meant according to the invention that the structure is brought into contact with the organic fluid through the major part, preferably almost all, of its outer surface. So a soaking does not necessarily mean immersion; it can be simply a contact with an organic fluid, partial or total. The dipping step (1) can be performed in one or more times, that is to say that the contact with the organic fluid can be carried out in one or more times. It allows the partial and controlled dissolution of a part of the lignin present in the material, that is to say a partial delignification. This allows both to retain enough lignin (native) within the material to maintain the micro-architecture of the wood, that is to say that it has a three-dimensional structure partially from the material before treatment , but it also allows to extract enough lignin through the organic fluid to release space in which will be inserted the filling compound and to prevent the presence of lignin within the structure limits the filling by the compound filling during the filling step (3). Such a limitation could strongly inhibit the propagation of the polymer chains by the action of hydroxyl groups (OH) which would block the radicals generated by a polymerization catalyst. This partial delignification excludes obtaining a fiber pulp of lignocellulosic material.
Of course, the amount of lignin extracted from the material depends on the very nature of this material, for example if it is a softwood or a hardwood.
Thus, in the case where the lignocellulosic material is softwood, it is generally from 50 to 85%, preferably from 50 to 75%, in weight%, of the lignin present in the structure which is dissolved at during the soaking step (1).
On the other hand, in the case where the lignocellulosic material is hardwood, it is generally from 40 to 60%, preferably from 45 to 55%, in% by weight, of the lignin present in the structure which is dissolved. during the soaking step (1).
For the conduct of the soaking step (1), the type of delignification does not matter as long as delignification makes it possible to retain the desired amount of lignin in the structure and does not significantly affect the micro-architecture of the lignin material. Cellulose that remains in place after extraction of the dissolved lignin is extracted. Thus, it may be a delignification by basic or acidic solution, by an ionic liquid, by an enzyme or by a bacterium. The enzyme or bacterium that can be used is generally carried by a fluid. which is more generally a liquid (in which case the fluid is generally a solution). However, it is preferred according to the invention delignification by at least one ionic liquid or at least one enzyme or at least one bacterium. The enzyme may be laccase, peroxidase, lignase or ATPase. Among the ATPases, mention may be made of the "copper-exporting P-type ATPase A" (copA). Among the peroxidases, mention may be made of "dye-decolorizing peroxidases" including those of type B (type Dyp-B), type P (type Dyp-type) and type 2 (type Dyp-2). It is alone or in a mixture of enzymes ("enzyme cocktail"). These enzymes can be secreted by a fungus in culture such as "white-rot fungi".
It should be noted that the role of enzymes can be twofold. Indeed, the partial delignification is "assisted" if the enzymatic action is that of the organic washing fluid. It is "completed" if the enzymatic action accompanies the action of the organic washing fluid, by reducing the solvated / dissolved elements derived from the lignin of the lignocellulosic material into elements of lower molecular weight.
Thus, the organic fluid of the dipping step (1) may be chosen from: an aqueous solution comprising a mixture of sodium chloride and sodium hydroxide, or an aqueous liquid comprising monoethanolamine, or a basic solution including KOH (for alkaline delignification); an aqueous solution comprising a mixture of acetic acid and hydrogen peroxide, or an acidic solution comprising HBr, H 2 SO 4 or H 3 PO 4 (for acid delignification); a fluid comprising at least one enzyme, optionally in the presence of at least one ionic liquid or in the presence of at least one ionic liquid and at least one co-solvent (for enzymatic delignification); a pure ionic liquid generally derived from the plant material (for delignification by pure ionic liquid); an ionic liquid containing one or more enzyme (s) in solution (for ionic liquid delignification assisted / supplemented by enzymatic action); an ionic liquid mixed with at least one solvent that is miscible with the ionic liquid, such as ethanol (for ionic liquid-assisted organosolv delignification, in which case the ionic liquid may be in the minority relative to the other or other miscible solvent (s) of this mixture); an ionic liquid mixed with at least one miscible solvent containing one or more enzyme (s) in solution; a bi-phasic system, one of the phases of which consists of an ionic liquid, pure or mixed with at least one miscible solvent, such as ethanol, and the other phase consists of a supercritical fluid, such as CO2 (for supercritical fluid delignification assisted by pure ionic liquid or mixture); a bi-phasic system, one of whose phases consists of an ionic liquid, pure or mixed with at least one miscible solvent, and the other phase consists of a supercritical fluid, containing in addition one or more enzyme (s) in solution in the phase containing the ionic liquid (for supercritical fluid delignification assisted by pure ionic liquid or mixture and assisted / supplemented by enzymatic action); any solution of a pure compound or a mixture of compounds containing at least one enzyme; and their mixtures.
In the preceding list relating to the organic fluid of the dipping step (1), the first compound of each element of this list is generally present mainly, that is to say at least 50% by weight. Any other compound cited and present in a minority way is different from this first compound.
But any other organic fluid capable of performing the desired function may also be considered by the skilled person, whether liquid or gaseous. Thus any enzyme or mixture of enzymes, or any fungus (such as "white-rot fungi") can facilitate the degradation of lignin within the material and thus lead to the partial delignification of this material.
By "supercritical fluid" is meant a fluid in the supercritical state. The supercritical fluid may be chosen from carbon dioxide CO2, alkenes with a low molecular weight (that is to say with a number of carbon atoms of at least 1 and strictly less than 5) such as ethylene or propylene, alkanes of low molecular weight (that is to say, with a number of carbon atoms of at least 1 and strictly less than 5) such as methane, ethane or propane, alcohols with a low molecular weight (that is to say with a number of carbon atoms of at least 1 and strictly less than 5) such as methanol or ethanol, nitrous oxide N 2 O, acetone, chlorofluoromethane, trichlorofluoromethane and ammonia. The soaking step (1) carrying out partial delignification can be carried out at ambient temperature, or with heating, at atmospheric pressure, under vacuum or under pressure, as is known to those skilled in the art. The addition of pressure and heat generally speeds up the hydrolysis process of lignin, which is particularly advantageous for industrial implementation.
By "ionic liquid" is meant according to the invention any solution of organic salt whose melting point is below 100 ° C., being generally liquid at ambient temperature, and having a low vapor pressure, that is to say boiling point between 200 ° C and 400 ° C.
A preferred ionic liquid according to the invention, used alone or as a mixture, is preferably chosen from imidazolium cationic ionic liquids (in which case the counterion is preferably selected from chloride, bromide, acetate, acesulfamate and mixtures thereof). ), even more preferably chosen from 1-alkyl-3-alkyl imidazolium, where the alkyls are, as is known, substituents derived from alkanes having lost a hydrogen atom, and wherein the alkyls each comprise independently from one to the other, from 1 to 6 carbon atoms per molecule, such as, for example, 1-butyl-3-methyl imidazolium or 1-ethyl-3-methyl imidazolium.
Thus, 1-ethyl-3-methylimidazolium bromide, 1-butyl-3-ethylimidazolium bromide, 1-butyl-3-methylimidazolium bromide, 1-ethyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium bromide. 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acesulfamate are preferred ionic liquids according to the invention.
The ionic liquid may also be synthesized from a molecule resulting from one of the lignocellulosic material treatment steps, in particular the delignification step. This advantageously makes it possible to optimize the by-products generated during the treatment process according to the invention. Thus, it is possible to envisage using ionic liquids synthesized from aromatic aldehydes derived from lignin or hemicellulose, such as vanillin, p-anisaldehyde or furfural, which are modified chemically, in particular to insert nucleophilic atoms therein. nitrogen. In this case, the ionic liquid according to the invention may also be chosen from ionic liquids with a cholinium cation, such as cholinium lysine. The advantage of using an ionic liquid is, in addition to the ease of use of such a product within the treatment process according to the invention, to be able to reuse it once it is extracted in a washing step (2). ) with the lignin dissolved and purified (that is to say rid of lignin and any other product including the organic washing fluid).
By "co-solvent" is meant according to the invention any liquid compound added in a small amount and miscible with another liquid, called primary or primary solvent. Such a co-solvent improves the solvation power of the primary solvent vis-à-vis the species that it is desired to dissolve. Generally, the main solvent is water to which is added a co-solvent which is a miscible organic solvent, such as acetone, ethanol, propanol or DMSO (for DiMethyl Sulfoxide).
According to a particularly preferred embodiment, the organic fluid of the dipping step (1) is a delignification liquid which further comprises at least one agent of polarity chosen from the group formed by ethanol, ethylene glycol, methyl ether, N-methyl pyrrolidone, dioxanes, dimethylformamide, diethylene glycol, diethylene glycol dimethyl ether, pyridine, n-butylamine, piperidine, morpholine, 4-picoline, 2-picoline , diethylamine, aniline, acetone, and methanol, as well as optionally at least one surfactant selected from the group consisting of ionic surfactants such as cationic, anionic and zwitterionic and nonionic surfactants.
The presence of such a polarity agent advantageously allows a better penetration of the filling compound within the lignin and cellulose structure of the material, during the subsequent filling step (3). According to a particularly preferred embodiment, the organic fluid of the soaking step (1) is a delignification liquid which further comprises at least one surfactant.
The surfactant is generally chosen from anionic surfactants such as those based on sulphate, sulphonate, carboxylate or phosphate esters; cationic surfactants such as quaternary ammonium salts; nonionic surfactants such as surfactants based on polyethylene oxide and / or polypropylene oxide, for example the family Pluronic® and Tween®, or based on fatty acid chain, for example the family of Span® and sugar; and zwitterionic surfactants such as amine oxides, for example lauramine oxide, betaines, alkyl amido betaines, sulfobetaines and imidazoline derivatives; and their mixtures. Lignin derived surfactants, such as those obtained by lignin sulfonation, may also be used.
For example, the dipping step (1) may for example be carried out under vacuum using an aqueous organic solution comprising from 5 to 10% of sodium chloride and from 0.01 to 0.5% of sodium hydroxide, at 50 to 90 ° C and for 2 to 10 hours, for example at 70 ° C for 5 hours. The washing step (2) allows extraction of the dissolved lignin present in the material following the soaking step (1). It can be carried out in one or several times, that is to say in several steps, until a satisfactory or even total extraction is obtained with respect to the amount of lignin dissolved in the dipping step (1). For example, if the extraction is carried out by means of successive washing steps with a liquid organic fluid, ie an organic solution, the extraction is carried out until a substantially free organic washing solution is obtained. of lignin.
The lignin which is dissolved and then extracted from the lignocellulosic material structure plays an essential role in the context of the process of the invention. Of course, other compounds can be dissolved and extracted or even simply extracted from the lignocellulosic material during the dipping (1) and washing (2) steps.
Preferably, the organic fluid of the washing step (2) is a liquid selected from the group consisting of ethanol, hexane, isopropanol, heptane and mixtures thereof.
For example, the washing step (2) can be carried out under vacuum with ethanol at 60 ° C for 4 hours.
But the washing step (2) can also be carried out by several successive baths of ethanol and hexane.
According to the process of the invention, the lignin extracted in the organic fluid from the washing step (2) is preferably used in a process for the recovery of lignin, generally on an industrial scale, for the manufacture of a material of a material or material used in aeronautics or a packaging material or a biofuel or a pharmaceutical compound or a chemical compound. We can thus use lignin to valorize it in carbon fiber (by aromatic combination), fiber-reinforced concrete, packaging, biofuels (by anaerobic digestion), drugs, and chemical components (ferulic acid in particular) and aromas (vanillin), but also for applications with higher added value such as the extraction of aromatic molecules as basic synthons in various fields of chemistry (polymers, synthesis of precursors ...) · Lignin can also be used through different pastes (kraft, pulp, alkaline paste, sulphite pulp ..) in the field of packaging. This confers on the process according to the invention an ecological process character (or "green" process), while avoiding the production of non-recyclable waste as much as possible.
It is thus possible within the scope of the invention, as has been envisaged in the literature, for uses of the lignin thus extracted from the organic fluid of the washing step (2) in fields as varied as : - biorefining (combustion products, synthetic gas, bioethanol); - biological specialty chemicals (aromatic derivatives such as vanillin, benzene, xylene, DMBQ (2,6-dimethoxy-1,4-benzoquinone), syringaldehyde, syringol, vanillic acid, sinapinic acid, p-hydroxybenzaldehyde, 3-ethylphenol 2-methylphenol, 3-methoxycatechol, ferulic acid, gases such as carbon dioxide, carbon monoxide, methane or methanol); - chemical specialties (low quality or medium quality carbon fiber for applications such as aerospace, automobile, motorcycles, airplanes, windmills, brakes, fishing rods ... asphalt additives, cement additives, and agents emulsifiers); and - miscellaneous and varied materials (plastic products such as phenolic resins, epoxy resins, lignin-polyurethane foams, rubber products such as lignin-polyurethane elastomer coatings, adhesives, chipboard products; animal nutrition such as tablets or binders; flammable products such as matches or barbecue liquids). The filling step (3) is a step during which filling by the filling compound of the partially delignified (and thus partially hollow) structure is carried out in the most efficient way possible. It can be performed in one or more times. Various techniques are possible for this filling, as is known to those skilled in the art.
In general, these techniques are of the series type (replacement of a fluid with another fluid in stages during a series, repeated several times, of successive impregnations, the concentrations of each fluid in the filling compound increasing exponential), by impregnation, by injection (by the RTM or RTM Light type vacuum for "Resin Transfer Molding"), by infusion (RIFT for "Resin Infusion under Flexible Tooling"), under vacuum or under pressure, in a reactor or an autoclave or a vacuum oven, or any other device that the skilled person knows able to perform this step.
The development of filling conditions is within the reach of the skilled person.
In the preferred case according to the invention of the use of an autoclave, it may be recommended to alternate vacuum phases with pressure phrases to impregnate the lignocellulosic material.
In an exemplary embodiment, the filling step (3) comprises a step of pressure impregnation of the partially delignified structure with a solution comprising the filling compound. This pressure is generally 0.1 to 2.5 MPa. The filling step (3) can also be carried out in an atmosphere without oxygen, either under vacuum or in the presence of dinitrogen, for a period of 20 to 24 hours with 500 ml of liquid composition of filling compound, at a constant temperature of 50.degree. ° C after heating to 80 ° C for one to two hours, the structure being immersed in a solution comprising the filling compound and the assembly being placed in a closed chamber at these temperatures. The filling step (3) of the treatment method according to the invention can be carried out essentially in two embodiments.
In a first embodiment, the filler is a polymer or a co-polymer.
In this case, the polymer or co-polymer is in the liquid state at the pressure and temperature conditions of the filling step (3), to perform the filling step (3) by soaking the partially delignified structure in the liquid polymer or co-polymer. Preferably the polymer or co-polymer is thermoplastic, and the temperature of the filling step (3) is greater than its glass transition temperature. In this case, the finishing step (4) consists of a resting at a temperature below the glass transition temperature of the polymer or co-polymer. This assumes that the polymer or co-polymer generally has a glass transition temperature higher than the subsequent use temperature, typically above about 25 ° C (room temperature).
Preferably, the polymer or co-polymer is selected from the group consisting of polyacrylates, polyamides (such as DuPont's Nylons®), polyesters, fluoropolymers (such as DuPont's Teflon®), polyethylene, polypropylene, polybutene, polystyrene, polyphenylene oxide, polyvinyl chloride, polyvinylidene chloride, polycarbonate, poly lactic acid, polyethersulfones, polyetherimides, polyaryletherketones ; as well as in the group formed by polymers and copolymers, not listed above and obtained from the monomers of the second embodiment, the list of which is given below.
In a second embodiment, the filling compound of the filling step (3) is a polymerizable monomer present in a monomeric solution.
In this case, the filling compound is a polymerizable monomer present in a monomer solution at the pressure and temperature conditions of the filling step (3), the monomer solution further comprising at least one catalyst.
In this case, the monomeric solution preferably comprises at least one monomer chosen from: - monomers from petroleum including methacrylates, such as butyl methacrylate, methyl methacrylate, ethyl methacrylate, glycidyl methacrylate tri-n-butyl tin methacrylate; acrylates such as ethyl acrylate; phthalates such as dialkyl phthalates wherein the alkyl comprises, for example, from 1 to 6 carbon atoms; nitriles such as acrylonitrile; styrene and styrenic derivatives such as t-butyl styrene and chorostyrene; vinyl compounds such as vinyl acetate, vinyl chloride and vinyl propionate; ethylenic compounds such as ethylene glycol or ethylene oxide; butadiene; isoprene; and - biobased monomers (i.e. of biological origin) including terpenes; glycerol and glycerol derivatives obtained after reaction with at least one of epichlorohydrin, isomers of propanediol and glycolic acid; derivatives of sugars; furfural derivatives (generally derived from the acidic depolymerization of hemicellulose); lactic and formic acid derivatives; monomers derived from castor oil (or "castor oil") such as sebacic acid; hydroxyalkanoic acids, such as those derived from formic, lactic and sebacic acids; bio-ethylene (or biological ethylene); bio-ethylene glycol (or biological ethylene glycol); bio-propylene (or biological propylene); bio-1,4-butanediol (or 1,4-butanediol biological); lignin derivatives, such as terephthalic acid; and their mixtures.
By "derivative of X" is meant according to the compounded invention synthesized from the compound X by a short sequence of chemical reactions essentially keeping the identity (that is to say the main chemical structure) of the compound X, such that an addition of a function or an increase of the carbon chain length (ie a carbon chain addition) or an oxidation or a reduction or a nucleophilic substitution or a ring opening. The advantage of using biosourced monomers is that it is possible to recover them later by recycling the composite material. This therefore makes it possible to obtain a partially or totally recyclable composite material, which confers on the process according to the invention an ecological process character (or "green" process).
According to one embodiment, the monomer is such that, once polymerized, it has substantially the same optical density as cellulose. The refractive index of the polymer thus obtained is typically in the range of 1.40 to 1.60, typically about 1.47.
According to one embodiment, the monomeric solution of the filling step (3) further comprises at least one agent of polarity selected from the group formed by ethanol, ethylene glycol, methyl ether, N-methyl pyrrolidone, dioxanes, dimethylformamide, diethylene glycol, diethylene glycol dimethyl ether, pyridine, n-butylamine, piperidine, morpholine, 4-picoline, 2-picoline, diethylamine, aniline, acetone, and methanol.
The presence of such a polarity agent advantageously allows a better penetration of the filling compound into the lignin and cellulose structure of the material, more precisely within the microfibrils so that the filling compound is grafted onto the cellulose.
According to another embodiment, independent or not of the previous embodiment, the monomeric solution of the filling step (3) further comprises at least one filler selected from the group consisting of clays, diamonds, marbles, glass, gypsum, limestone, mica, perlite, quartz, sand, talc and their mixtures.
According to one embodiment, the filling compound consists of two monomers which lead to the manufacture of a thermosetting polymer in the finishing step (4), which consists of polymerization and crosslinking.
An example of a second embodiment is that the filling step (3) comprises a diffusion step comprising a first sub-step of immersing the partially delignified structure in a mixture of 50% of the monomer solution and 50% of the monomer solution. ethanol, then a second substep of immersion of the structure resulting from the first substep in a mixture of 75% of the monomer solution and 25% of ethanol, then a third substep of immersion of the structure resulting from the second substep in a mixture of 100% of the monomer solution, then a fourth sub-stage of immersion of the structure resulting from the third substep in a mixture of 100% of the monomer solution and of catalyst, each substep of immersion being carried out at room temperature for 24 hours.
Preferably, the catalyst is selected so as to catalyze a radical polymerization reaction, and this choice depends, in addition to the monomer, the mode of polymerization and its control. The catalyst is preferably selected from the group consisting of azo compounds of formula RN = N-R 'where R and R' are alkyl groups optionally comprising at least one additional function, such as azoisobutyronitrile, peroxides, halogenated alkyl compounds (generally comprising 1 to 6 carbon atoms per molecule) (that is to say comprising a halogen atom, namely chlorine, bromine, iodine or fluorine), nitroxides, the thio-carbonyl-thio compounds. But any other compound known to those skilled in the art as a catalyst is also possible.
According to one embodiment, the filling step (3) may advantageously be carried out in the presence of a neutral gas such as dinitrogen or argon or of a supercritical compound (i.e. in the supercritical state).
The neutral gas advantageously makes it possible to avoid the evaporation of the filling compound during the filling (3) and finishing (4) stages, as well as to avoid the contact of said compound with the ambient air, and in particular the oxygen of the air. The supercritical state is a state in which the contact angle of the compound with a substrate is zero, which implies that the compound wets its substrate completely: thus, the supercritical compound makes it possible to assist the lignocellulosic material. to be filled by the filling compound. The finishing step (4) is a step in which the filling compound of the partially delignified filled structure resulting from the filling step (3) is fixed in the structure, which makes it possible to obtain a structure of composite material formed of a three-dimensional network of converted filling compound incorporated into a cellulose and lignin network. It can be performed in one or more times.
It is carried out in different ways, in particular according to the embodiment of the filling step (3).
Thus, when the filling step (3) is carried out according to the first embodiment, that is to say that the filling compound is a polymer or a co-polymer preferably thermoplastic, the finishing step ( 4) consists in freezing (or fixing), as far as possible, the polymer or copolymer within the structure for its subsequent use. In other words, the finishing step (4) consists of putting said polymer or co-polymer in a physical state such that it can hardly leave the structure under the conditions of temperature and pressure considered. These temperature and pressure conditions essentially depend on the subsequent use to be made of the composite material structure, ie typically if it is intended to be placed outdoors (in which case the climate of the place of use should be taken into consideration) or indoors. In general, this results in a temperature lower than the glass transition temperature of the polymer or co-polymer.
Thus, when the filling step (3) is carried out according to the second embodiment, that is to say that the filling compound is a polymerizable monomer present in a monomeric solution, the finishing step (4) is to polymerize the monomer in the presence of the catalyst. This is generally done by any conceivable polymerization technique, such as the thermal pathway, the UV path, or the plasma route. The choice of the technique depends essentially on the nature of the polymerization catalyst, as is known to those skilled in the art.
For example, the monomeric solution comprises butyl methacrylate and styrene in proportion of one part of butyl methacrylate to 3 parts of styrene, and the catalyst present in the finishing stage (4) is razoisobutyronitrile at a rate of 0 , 05 part. In this case, the finishing step (4) can be carried out by heating at a temperature of 15 ° C. to 80 ° C., for example 40 ° C., under vacuum or under an atmosphere devoid of oxygen, for example under a free atmosphere. oxygen for 20 to 50 hours, for example for about 24 hours.
When the polymer or co-polymer obtained is thermosetting, the filling step (3) was carried out in the liquid state and at a temperature higher than the temperature range at which the crosslinking is set up and said polymer or co -polymer begins to harden. Then, the finishing step (4) consists of a polymerization then crosslinking of the source monomers of the thermosetting polymer, at a temperature below said temperature range of the polymer or co-polymer.
According to the invention, the treatment method may further comprise a step of pressurizing (5) the structure resulting from the finishing step (4). The pressurization step (5) is typically carried out at 80 to 250 ° C for 5 to 30 minutes at a pressure of 0.1 to 2.0 MPa.
This pressurization step (5) may be followed by a surface finishing step (or surface treatment) (6) of the structure resulting from the pressurization step (5). The surface finishing step (6) can typically be carried out chemically, for example by means of ethyl acetate, or by thermal see and accompanied by a press, in which case the steps of pressurizing (5) and surface finish (6) are performed simultaneously. This advantageously makes it possible to smooth out the surface irregularities of the structure. The subject of the invention is also, in a second aspect, a composite material structure comprising lignin, hemicellulose, cellulose and at least one filling compound, said structure being capable of being obtained, preferably obtained, by the implementation of the treatment method according to the invention, wherein the composite material forms a three-dimensional network of converted filling compound incorporated into a cellulose and lignin structure.
The structure of composite material according to the invention is generally advantageously a structure of good fire resistance, increased relative to the lignocellulosic material before treatment, rotproof, of improved durability compared to the lignocellulosic material before treatment, and has improved mechanical properties of compressive and flexural strength over lignocellulosic material prior to treatment. Of course, these properties depend inter alia on the nature of the filling compound.
According to a preferred mode of relationship, the composite material structure has substantially, or almost all, a substantially homogeneous refractive index.
Preferably, the composite material structure is substantially translucent. This optical property is advantageously obtained by homogenization of the optical index of the monomeric solution with that of the cellulose (in particular alpha cellulose). This advantageously provides the structure with additional optical quality because the light is transmitted through this composite material structure in a substantially homogeneous manner if this refractive index is substantially that of the cellulose.
Typically, the composite material structure comprises at least one dimension of at least 2 mm and at most 40 cm. This does not generally correspond strictly to the dimensions of the structure before treatment according to the method of the invention. Indeed, it is possible that a decrease of at least one of the dimensions of the structure occurs during the treatment process, particularly when it comprises a step of pressurizing (5) the structure.
The composite material structure obtained according to the method of the invention is preferably a finishing element, a finishing element or an element of first work. Finally, the invention relates, in a third aspect, a part comprising at least one composite material structure according to the invention, said part being a piece of furniture or a piece of furniture, a building element, a car part or an aeronautical part.
The room can be used in a wide variety of outdoor uses, in which case the room is generally selected from soffits, window frames, door and door frames, verandahs, planks, garden sheds terraces and half-timbered buildings and the like. Alternatively, the piece can be used in a wide variety of indoor uses, in which case the piece is generally selected from furniture, carpentry products and food containers such as food bowls. The invention will be better understood in view of the accompanying drawings, in which: FIG. 1 schematically represents the principle of the treatment method according to the invention; - Figure 2 shows schematically an example of partial implementation of a process step of the method according to the invention, said step comprising immersing the structure of lignocellulosic material in a liquid; - Figure 3 schematically shows an example of implementation of the pressurizing step of the method according to the invention; FIG. 4 diagrammatically represents an example of complete implementation of the filling step (3) and of the finishing step (4) of the process according to the invention, in the case where these steps involve the immersion of the structure of lignocellulosic material in a liquid according to Figure 2; - Figure 5 shows schematically a scanning electron microscope (SEM or SEM) view of a longitudinal section of wood in its natural state; - Figure 6 schematically shows a macroscopic three-dimensional view of a wood structure in the natural state (or native) before treatment according to the invention; FIG. 7 schematically represents a three-dimensional microscopic view of the wood structure in the natural (or native) state, before treatment according to the invention, of FIG. 6; - Figure 8 shows schematically an intermediate scale view of the wood structure, after the steps of dipping (1) and washing (2) according to the invention, Figures 9 and 10; - Figure 9 schematically shows a three-dimensional macroscopic view of the wood structure of Figures 6 and 7 after the steps of dipping (1) and washing (2) according to the invention; Figure 10 schematically shows a three-dimensional microscopic view of the wood structure of Figure 9; - Figure 11 schematically shows a three-dimensional macroscopic view of the wood structure of Figures 9 and 10 after the step of filling with a filling compound (3); Figure 12 schematically shows a three-dimensional microscopic view of the wood structure of Figure 11; 13 schematically represents a macroscopic three-dimensional view of the wood structure of FIGS. 11 and 12 after the finishing step (4), that is to say of the composite wood structure obtained by the method of FIG. treatment according to the invention; Figure 14 schematically shows a three-dimensional microscopic view of the composite wood section of Figure 13; FIG. 15 shows three scanning electron microscope (SEM) photographs on a semi-microscopic scale of a fir structure part at different stages of the treatment method according to the invention, namely from left to right respectively before treatment delignification, after delignification and before impregnation with a monomeric compound, and after polymerization of the monomeric compound thus impregnated; FIG. 16 shows two photographs by scanning electron microscope (SEM) after partial enlargement of the fir structure part of FIG. 15, that is to say on a microscopic scale, namely from left to right respectively before treatment and after polymerization of the impregnated monomeric compound; - Figure 17 shows the block diagram of the bending of a wood structure treated by a method according to the invention; - Figure 18 illustrates the result of measuring the bending of a fir structure, before and after treatment; FIG. 19 represents the principle diagram for measuring the axial compression of a wood structure treated by a method according to the invention; FIG. 20 illustrates the measurement result of the axial compression of a fir structure, before and after treatment; - Figure 21 shows the principle diagram for measuring the axial tension of a wood structure treated by a method according to the invention; FIG. 22 illustrates the measurement result of the axial traction of a fir structure, before and after treatment; and - Figure 23 shows ten photographs by Zeiss LSM710 Upright microscope after treatment of six different wood species.
Figure 1 shows schematically the treatment method according to the invention, by successive steps, each being represented by a box. Each of the boxes corresponds to the step bearing the same reference number of the method according to the invention, it being understood that references (5) and (6) are optional steps as shown by the dashed arrows connecting the boxes 4, 5 and 6.
There is thus distinguished, in order, a first step (1) which is a step of soaking the lignocellulosic material structure. Step (1) performs a partial extraction of lignin from this structure. It is followed by a second step (2) which is a washing step of the structure resulting from step (1), to evacuate the dissolved lignin from step (1). This washing step (2) is followed by a third step (3) of filling the partially delignified structure resulting from the washing step (2) with at least one filling compound. The last and fourth step (4) is a step of fixing the filling compound in the structure resulting from the filling step (3). This makes it possible to obtain a composite material structure formed of a three-dimensional network of transformed filling compound incorporated into a cellulose and lignin network. This fourth step may be followed by a fifth step (5) of pressurizing the structure resulting from the finishing step (4), possibly itself followed by a sixth surface finishing step (6) of the structure (10) from step (5).
Figure 2 shows schematically an example of partial implementation of a process step of the method according to the invention, said step comprising immersing a structure of lignocellulosic material (10) in a liquid. The structure of lignocellulosic material illustrated is a structure of wood, for example fir. It is immersed in a treatment solution (11), which can be an organic solution of the soaking step (1), an organic solution of the washing step (2) or a solution comprising at least one filling compound of the filling step (3). The assembly rests on a support (15), for example Teflon, which is itself fixed in a tray (12), for example stainless steel.
Figure 3 schematically shows an example of implementation of the optional step of pressurizing (5) of the method according to the invention. In this case, the composite material structure (10 ') is compressed within a compression apparatus (13, 14) composed of two symmetrical jaws (13) and (14) that can be brought closer to each other by taking the intermediate structure (10 ') in vice. On each of the parts (13) and (14) is exerted an axial force opposite the force exerted on the other part (the two forces being represented by arrows), thus bringing them closer to each other.
FIG. 4 diagrammatically represents an example of complete implementation of the filling step (3) and the finishing step (4) of the method according to the invention, in the case where these steps comprise the immersion of the structure of lignocellulosic material in a liquid according to Figure 2.
In this Figure, the assembly shown in Figure 2 is disposed within an enclosure (25). More specifically, the tray (12) is fixed in the enclosure (25) by means of a metal support (16). The enclosure (25) is such as to control the pressure and temperature conditions that are present within it. These conditions depend mainly on the nature of the filling compound. The enclosure (25) may be a vacuum oven or an autoclave.
A pipe (22), which is divided into a pipe (22a) and a pipe (22b), allows, by means of the respective valves (17) and (18), respectively to evacuate or to introduce nitrous nitrogen N2. within the enclosure (25).
A pipe (23), which is divided into a pipe (23a), a pipe (23b), a pipe (23c) and a pipe (23d), allow, by means of the respective valves (19), (20), 21) and (26), to evacuate or introduce into the chamber a respective solution (24a), (24b), (24c) or (24d). A pure solution (24a), (24b), (24c) or (24d), or a possible mixture of at least two of these solutions (24a), (24b), (24c) and (24d), thus constitutes the treatment solution (11) (which may vary according to the step or substep of the process), in which the wood structure (10) is embedded. This allows, for performing the filling step (3), to conduct a treatment of the wooden structure (10) in series, each series comprising successive immersions for example in the order of use of the solutions. The processing step (3) usually comprises several series, typically from 2 to 6 series, for example 4 series.
Of course, it is possible to provide alternatively the device shown in Figure 4 another device comprising as many organic treatment solutions as necessary, each treatment solution being associated with a pipe on which is present a valve, connected to the pipe (23) in direct relationship with the enclosure (25).
Figure 5 shows schematically a scanning electron microscope (SEM) view of a longitudinal section of a wood structure, for example walnut, in the natural state. We can see the micro-architecture of the wood. At this scale, there are cavities (or "lumen") (28) of cellulose delimited by the walls (27) formed of cellulose fibers, and the transverse perforations forming pores or channels (29) between the cell cavities. These cell cavities have a transverse dimension of 30 to 60 pm for softwoods and 70 to 350 pm for hardwoods. The transverse perforations (29) represent areole-shaped pits for softwood or substantially circular holes for hardwood, the transverse dimension of which varies from about 6 to about 30 microns, and averages about 15 microns. Figure 5 corresponds substantially to a section in the longitudinal direction of the structure shown schematically in Figure 6.
Figures 6 and 7 show schematically two views in three dimensions, respectively macroscopic and microscopic, of a wood structure in the natural state (or native), that is to say before treatment according to the invention. It contains the cavities (28) of medium-sized wood in the transverse direction of about 75 μηι, with disparities depending on the nature of the wood, to be about 30 to about 60 μm for softwoods, and about 70 to about 350 pm for hardwoods. These cavities (28) are delimited by cell walls of average thickness of about 2 to about 10 microns for softwoods and hardwoods.
As can be seen in FIG. 7, the micro-architecture of the wood from which its natural strength derives comes from all the walls of the cellular cavities (28) which consist of tubes or microfibrils (45). , themselves formed into bundles or macrofibrils (47). The macrofibrils (47) are chemically bonded to transverse hemicellulose support structures (46), chemically bonded transversely to longitudinal lignin support structures (44), which assembly (46, 44) serves as a support macrofibrils (47) of cellulose.
Figures 8, 9 and 10 show schematically three views in three dimensions, respectively at the intermediate scales between macroscopic and microscopic, macroscopic and microscopic, of a wood structure after the steps of soaking (1) and washing (2) according to the 'invention.
The cell wall (49), which has thinned with respect to that shown in Figures 6 and 7, is distinguished. The thickness of the cell wall (49) is from about 2 to about 10 μm, averaging about 6 pm. Microfibrils (45), hemicellulose (46) and macrofibrils (47) are substantially unchanged from Figures 6 and 7. Lignin (44 ') is still present but "lightened", that is to say in a smaller amount than the lignin (44) shown in Figures 6 and 7.
Figure 8 details the cell wall 49, on a junction of walls (see Figure (9)). The cell wall (49) of cellulose comprises a mean lamella (61) with a thickness of about 0.2 to about 1 μm, as well as two walls, the primary wall (55) having a thickness of about 0.1 μm. , and the secondary wall (60), itself consisting of three sub-layers respectively (52), (53) and (54) in the direction of the cavity (28) towards the outside, the first sub-layer ( 52) having a thickness of about 0.1 to about 0.2 μm, the second underlayer (53) being about 1 to about 5 μm thick and the third underlayer (54) being about thickness from about 0.1 to about 0.2 μm. There is also a transverse perforation (29), which consists of an orifice proper (50), of average size of about 0.02 to 4 μm, surrounded by a perforation (51), of average about 6 to 30 pm.
During the partial delignification carried out by the soaking step (1) associated with the washing step (2), the primary wall (65) and the third sub-layer (54) of the adjoining secondary wall (60) have They were the most delignified, being themselves the most lignin-laden layers or sub-layers, the third sub-layer (52) itself having very low lignin content, having practically not been delignified. This explains the differences in dimensional variations within the lignocellulosic material structure that occur during partial delignification according to the invention. Note that Figure 8 could also illustrate, by adapting the dimensions indicated above, the material before treatment during the processing steps that are the steps of soaking (1) and washing (2) of the method according to the invention. invention. Indeed, during these steps, the only change found comes from the thickness of some of the layers and underlays as explained above, which is reduced as and treatment.
Figures 11 and 12 schematically show two three-dimensional views, respectively macroscopic and microscopic, of the wood structure of Figures 9 and 10 after the step of filling with a filling compound (3). It contains the microfibrils (45), the lightened lignin structure (44 '), the hemicellulose structure (46), the macrofibrils (47), and the walls (49) of the cavities (57). These cavities (57) are now filled with filling compound, forming a three-dimensional filling network (58). In practice this amounts to filling the macrofibrils and their interstices with this filling compound, and possibly filling the microfibrils with the filling compound according to the degree of penetration of the filling compound into the material.
Figures 13 and 14 schematically show two three-dimensional views, respectively macroscopic and microscopic, of the wood structure of Figures 11 and 12 after the finishing step (4) (generally consisting of polymerization). They thus schematically illustrate the composite wood structure obtained by the treatment method according to the invention. It contains the microfibrils (45), the lignin lignin structure (44 '), the hemicellulose structure (46), the macrofibrils (47), and the walls (49) of the three-dimensional filling network (59).
Figures 15 to 23 are explained in the examples below. The invention will be better understood from the following examples of embodiments, with reference to the accompanying drawings.
EXAMPLES
The examples which follow illustrate the invention without limiting its scope.
Example 1; Method of treatment according to the invention of a fir structure
A parallelepipedic sample of fir wood measuring 0.5 cm × 4 cm × 8.5 cm (I × L × h) was subjected to the treatment method according to the invention, which made it possible to obtain, in the course of experiments of laboratory, a composite specimen of dimensions 0.45 cm x 3.6 cm x 8.2 cm (IxLxh). The chamber used was a vacuum oven (25).
Thus, the sample was treated during a first soaking step (1) by means of three identical successive sub-steps, each consisting of immersing the sample in a solution of 6% sodium chloride and 0.05% sodium hydroxide under vacuum at a constant temperature of 70 ° C for 5 hours. The Savage step (2) of the sample was then implemented, by immersing the sample resulting from the preceding dipping step (1), by means of 4 identical first successive substeps, each consisting of immersing the sample from the preceding step or substep in a 99% ethanol solution, under vacuum, at a constant temperature of 60 ° C for 4 hours, followed by 3 second substeps identical successive ones, each consisting of immersing the sample from the previous substep in a 99% hexane solution, under vacuum, at a constant temperature of 50 ° C for 3 hours. The sample from the washing step (2) was then allowed to stand so that the hexane still present in the wood sample evaporated for a period of 2 hours.
The steps of filling (3) and finishing (4) of the sample thus obtained were carried out by means of the device shown in FIG. 4. The filling step (3) was carried out according to the second embodiment, by vacuum impregnation. Thus, a "primary" monomeric solution consisting of one part of butyl methacrylate and three parts of styrene was produced after the purification of these compounds with a filtering powder made of diatomite. The primary monomeric solution was mixed for a first series, at 50% by volume for 50% ethanol. The primary monomeric solution was mixed, 75% for 25% ethanol, for a second series. The primary monomeric solution (100%) was the solution of the third series. The primary monomeric solution (95%), added to 0.05 parts of catalyst (asoisobutyronitrile), constituted the solution of the fourth series. The filling step (3) thus comprised four series, each series comprising four successive sub-steps, successively by the following solutions, made from the solutions of the fourth series solution (monomer solution + catalyst) (24a), ethanol (24b), hexane (24c) and monomer solution (24d), without manipulation of the structure (10) and without contact with the air. The treatment of this step (3) was carried out under vacuum and at room temperature, for a period of 24 hours per series. At the end of the filling step (3), the solution (11) was drained by releasing the vacuum (17) and blowing the dinitrogen (18) to saturate the volume of the enclosure (25), which has advantageously prevented the evaporation of the monomers present in the structure (10). The finishing step (4) which followed was a polymerization stage of the butyl methacrylate and styrene monomers filling the sample at the end of the filling step (3). This polymerization, leading to the formation of co-polymer butyl methacrylate-styrene, was carried out under vacuum, for a period of 20 to 24 hours for 500 ml of monomer solution (11) at a temperature of 80 ° C. for both first hours then 50 ° C for the rest of the stage.
This finishing step (4) was followed by a pressurization step (5) which was carried out in the device of FIG. 3. The sample resulting from the finishing step (4) was wrapped between two sheets of latex 0.7 mm thick each, the two sheets completely covering the sample and thus overlapping on all four edges. They created a pocket that conformed to the shape of the sample. This bag was then evacuated using a valve, the container-content assembly thus forming the structure (10 '). The whole was placed in an oven at a temperature of 40 ° C for a period of 24 hours. The pressurizing step (5) was followed by a demolding step of the wood composite structure thus obtained from the pocket, and then a surface finish during a surface finishing step ( 6) with a light jet of ethyl acetate. The thus obtained composite fir sample was translucent.
It is also possible to provide a variant where the enclosure (25) is an autoclave (25), in which case a single series may be sufficient to perform the filling step (3), the finishing step (4) is performed by immersion in a bath and the steps of pressurizing (5) and surface finishing (6) are then not necessary. Example 1 was carried out several times, in order to obtain several composite fir samples which were evaluated in destructive mechanical tests and in non-destructive optical tests, as explained in Example 2 below. .
EXAMPLE 2 Evaluation of the Structure of Composite Spruce Resulting from the Treatment Process According to the Invention and Obtained in Example 1
The fir tree composite fir sample obtained in Example 1 was evaluated both for its strength properties and also for its optical properties.
Mechanical tests illustrated in Figures 17 to 22
Bending measurement illustrated in Figures 17 and 18
This measurement was carried out on fir specimens measuring 0.7 cm × 2.5 cm × 10 cm (× 1 × h), according to a method developed by the applicant comprising three identical pulleys (39), of 3 cm in diameter. , exerting a flexion on the structure. These three pulleys (39) were spaced two by two by 3 cm, the distance between the two pulleys (39) farthest being 7 cm.
FIG. 17 represents the basic diagram for measuring the bending of the fir sample forming a composite fir structure (38) according to the invention.
As seen in Figure 17, a force F was applied to the sample, increasingly stronger, perpendicular to its main plane, and the maximum stress just before breaking (arrow f) was measured.
Figure 18 illustrates the result of this measurement of bending of the fir sample, before treatment (curve A) and after treatment (curve B).
For the natural (or native) fir sample (curve A), the maximum stress at break was measured at 175 kgf / cm2, and the deflection deflection was 0.53 cm.
In contrast, for the translucent composite fir sample according to the invention (curve B), the maximum stress at break was measured at 350 kgf / cm 2, and the deflection sag was 0.65 cm.
Thus, the cellular densification of the fir tree thanks to the treatment according to the invention has made it possible to withstand an increased bending force of 200%. In addition, unlike the native fir, the break is more progressive in the case of composite fir material according to the invention. As a result, the material has gained ductility through the treatment of the invention. Without wishing to be bound by any theory, the inventor believes that this is probably due to a strong adhesion between the fibers and the polymeric matrix.
Axial compression measurement illustrated in Figures 19 and 20
This measurement was carried out on fir samples of dimensions 1 cm × 3.5 cm × 10 cm (I × W × h), according to a method developed by the applicant.
Figure 19 represents the schematic diagram of the measurement of the axial compression of the fir sample forming structure (41) of composite fir according to the invention.
As can be seen in FIG. 19, a compression force F has been applied to the sample (41) by a crushing plate (40) of 7 cm in diameter, more and more strong, parallel to its main axis, and the maximum stress just before breaking (distance da) was measured.
Figure 20 illustrates the result of this measurement of axial compression of the fir sample, before treatment (curve A) and after treatment (curve B).
For the natural (or native) fir sample (curve A), the maximum tensile strength at break was measured at 254 kgf / cm2, and the deformation just before breaking was 0.959 cm.
On the other hand, for the translucent composite fir sample according to the invention (curve B), the maximum stress at break was measured at 430 kgf / cm 2, and the deformation just before breaking was 0.978 cm.
Thus, the cellular densification of the fir tree thanks to the treatment according to the invention has made it possible to withstand an increased axial compression force of 170%. In addition, unlike the native fir, the break is more progressive in the case of composite fir material according to the invention. Without wishing to be bound by any theory, the inventor thinks that this is probably due to the nature of the composite fir, which leads to the appearance of a crack in the matrix being stopped by wood fibers reinforced by the polymer.
Axial tensile measurement illustrated by Figures 21 and 22
This measurement was carried out on fir samples measuring 0.2 cm × 3 cm × 7.5 cm (I × L × h), according to a method developed by the applicant.
FIG. 21 represents the principle diagram for measuring the axial tension of the fir sample forming a composite fir structure (43) according to the invention.
As can be seen in FIG. 21, two identical forces of opposite traction direction F have been applied to the sample via two identical claws (42), which are stronger and stronger, parallel to its main axis. and the maximum stress before failure was measured. Each claw (42) had dimensions 1.5 cm x 2.5 cm x 1 cm (IxLxh).
Figure 22 illustrates the result of this measurement of axial traction of the fir sample, before treatment (curve A) and after treatment (curve B).
For the natural (or native) fir sample (curve A), the maximum breaking stress was measured at 125 kgf / cm2, and the extension just before breaking was 0.7 cm.
In contrast, for the translucent composite fir sample according to the invention (curve B), the maximum stress at break was measured at 165 kgf / cm 2, and the extension before rupture was 0.7 cm.
Thus, the recorded plastic deformation was about 6% before breaking. The behavior of the material according to the invention to the axial tensile force is therefore substantially identical to that of the material before treatment. There is no deterioration of this value by the use of the method according to the invention.
Optical tests illustrated by Figures 15, 16 and 23
The composite fir structure obtained in Example 1 was translucent.
Figures 15 and 16 show, at two different scales of scanning electron microscope (SEM) photographs of a part of fir wood structure treated in Example 1, at different stages of the treatment process according to the invention.
FIG. 15 shows three photographs by scanning electron microscope (SEM) of a part of fir wood structure at different stages of the treatment method according to the invention, namely from left to right respectively before delignification treatment (natural wood or native), after delignification and before impregnation with a monomeric compound, and after polymerization of the monomeric compound thus impregnated. Figure 16 shows two photographs by scanning electron microscope (SEM) after partial enlargement of the fir tree structure part of Figure 6, before from left to right respectively before treatment (natural or native wood) and after polymerization of the compound impregnated monomer.
The clear parts which fill up after impregnation of the filling compound, are different after the impregnation, especially whiter and wider (see the comparison between parts 30 and 31 of Figure 15, as well as between parts 36 and 34 of Figure 16).
The dark portions (32 for the second photograph in Figure 15, 33 for the third photograph in Figure 15, 37 for the first photograph in Figure 16 and 35 for the second photograph in Figure 16) correspond to air and could be significantly reduced by further optimization of the process. These photographs show the disordered state of the wood before delignification, which does not allow to distinguish the cavities of the cells, the more orderly state of the wood after delignification, where one clearly distinguishes the cavities of the cells, and the state wood cavities partially filled by the polymer, after the treatment process according to the invention. It can thus be seen that the composite wood obtained after the treatment process according to the invention is strongly structured in accordance with the original micro-architecture of the wood: the walls of the cells which consisted mainly of cellulose have been transformed into walls in which they have been inserted pellets of polymer and the polymer at least partially filled the cell cavities.
Figure 23 shows two photographs by Zeiss LSM710 Upright microscope with an objective x 20 of the composite fir structure, in longitudinal radial section (CLR) and in cross section (CT). The ambient lighting is 257 lux.
The first photograph is in radial longitudinal section (CLR) obtained with 14 lux of direct light transmission for the ambient lighting considered (ie 5.5% of light transmission), while the second photograph of this sample is in plane of cross section (CT) obtained with 27 lux of direct light transmission for the ambient lighting considered (ie 11% of light transmission).
These 2 photographs show that the composite wood is a 3-dimensional structure that is to say that whatever the cutting plane, the translucent nature of the composite fir appears.
Example 3: Optical evaluation of composite structures of white pine, white oak, acaiou. of linden and ash resulting from a treatment process according to the invention obtained as in Example 1
The treatment method of Example 1 was reproduced on other species, namely on samples forming composite structures of five species: white pine, white oak, mahogany, linden and ash. The optical optical transmission properties of the samples of these five different wood species were evaluated.
Figure 23 shows eight Zeiss LSM710 Upright microscope photographs with an x 20 objective of composite wood structures made from these five species.
The first photograph of the white pine sample is in radial longitudinal sectional plane (CLR) obtained with 20 lux of direct light transmission for the ambient lighting considered (ie 8% of light transmission), while the second photograph of this sample is in cross-sectional (CT) plane obtained with 65 lux of direct light transmission for the ambient lighting considered (ie 25% of light transmission).
The only photograph of the white oak sample is in cross-sectional (CT) plane obtained with 22 lux of direct light transmission for the ambient lighting considered (ie 9% of light transmission).
The only photograph of the mahogany sample is in cross-sectional (CT) plane obtained with 33 lux of direct light transmission for the ambient lighting considered (ie 13% of light transmission).
The first photograph of the basswood sample is in radial longitudinal sectional plane (CLR) obtained with 30 lux of direct light transmission for the ambient lighting considered (ie 12% of light transmission), while the second photograph of this sample is in cross-sectional plane (CT) obtained with 70 lux of direct light transmission for the ambient lighting considered (ie 30% of light transmission).
The first photograph of the ash sample is in radial longitudinal sectional plane (CLR) obtained with 11 lux of direct light transmission for the ambient lighting considered (ie 4.3% of light transmission), while the second photograph of this sample is in cross-sectional (CT) plane obtained with 33 lux of direct light transmission for the ambient lighting considered (ie 13% of light transmission).
In each case, these photographs show that the composite wood is a three-dimensional structure that is to say that whatever the cutting plane, the translucent nature of the composite wood appears.
It would be possible to significantly improve the light transmission of the composite wood by refining the process by those skilled in the art, particularly as regards the control of the delignification, the saturation / filling depth and the nature of the filling compound whose index Once transformed, the refractive index must be almost homogeneous with the refractive index of the composite lignocellulosic substrate.
权利要求:
Claims (15)
[1" id="c-fr-0001]
A method of treating a lignocellulosic material structure, the lignocellulosic material preferably being wood, said method comprising the following steps: (1) at least one step of dipping the lignocellulosic material structure by an organic fluid to dissolve at least 40% and at most 85% wt% of the lignin present in the material; (2) at least one step of washing the structure resulting from step (1) by at least one organic fluid so as to evacuate the dissolved lignin resulting from the soaking step (1), so as to produce a structure partially delignified; (3) at least one step of filling the partially delignified structure resulting from the washing step (2) with at least one filling compound, so as to produce a partially delignified filled structure; and (4) at least one step of finishing the partially delignified filled structure resulting from the filling step (3), so as to obtain a composite material structure formed of a three-dimensional network of transformed filling compound incorporated into a cellulose and lignin network.
[2" id="c-fr-0002]
The method of treatment of claim 1, wherein the lignocellulosic material structure is a finishing element, a finishing element or a first work element.
[3" id="c-fr-0003]
3. Treatment method according to one of claims 1 and 2, wherein the organic fluid of the soaking step (1) is selected from: an aqueous solution comprising a mixture of sodium chloride and sodium hydroxide, or an aqueous liquid comprising monoethanolamine, or a basic solution comprising KO H; an aqueous solution comprising a mixture of acetic acid and hydrogen peroxide, or an acidic solution comprising HBr, H2SO4 or H3PO4; a fluid comprising at least one enzyme, optionally in the presence of at least one ionic liquid or in the presence of at least one ionic liquid and at least one co-solvent; A pure ionic liquid; an ionic liquid containing one or more enzyme (s) in solution; an ionic liquid in admixture with at least one solvent miscible with the ionic liquid; an ionic liquid in admixture with at least one miscible solvent containing one or more enzyme (s) in solution; a bi-phasic system, one of which consists of an ionic liquid, pure or mixed with at least one miscible solvent, and the other phase consists of a supercritical fluid; a bi-phasic system, one of whose phases consists of an ionic liquid, pure or mixed with at least one miscible solvent, and the other phase consists of a supercritical fluid, containing in addition one or more enzyme (s) in solution in the phase containing the ionic liquid; and any solution of a pure compound or a mixture of compounds containing at least one enzyme; and their mixtures.
[4" id="c-fr-0004]
The treatment method according to one of claims 1 to 3, wherein the organic fluid of the soaking step (1) is a delignification liquid which further comprises at least one polarity agent selected from the group consisting of ethanol, ethylene glycol, methyl ether, N-methyl pyrrolidone, dioxanes, dimethylformamide, diethylene glycol, diethylene glycol dimethyl ether, pyridine, n-butylamine, piperidine, morpholine, 4-picoline, 2-picoline, diethylamine, aniline, acetone, and methanol, as well as optionally at least one surfactant selected from the group consisting of ionic surfactants such as cationic, anionic and zwitterionic and nonionic surfactants.
[5" id="c-fr-0005]
5. Treatment process according to one of claims 1 to 4, wherein the organic fluid of the washing step (2) is a liquid selected from the group consisting of ethanol, hexane, isopropanol, heptane and their mixtures.
[6" id="c-fr-0006]
The treatment method according to one of claims 1 to 5, wherein the filling compound of the filling step (3) is in the liquid state at the pressure and temperature conditions of the filling step ( 3), to perform the filling step (3) by soaking the partially delignified structure in the liquid polymer or co-polymer.
[7" id="c-fr-0007]
7. Treatment method according to one of claims 1 to 7, wherein the filling compound of the filling step (3) is a polymerizable monomer present in a monomer solution at the pressure and temperature conditions of the step filling (3), the monomeric solution further comprising at least one catalyst.
[8" id="c-fr-0008]
8. Treatment process according to claim 7, wherein the monomer solution of the filling step (3) comprises at least one monomer chosen from: monomers from petroleum including methacrylates; phthalates; nitriles; styrene and styrenic derivatives; vinyl compounds; ethylenic compounds; butadiene; isoprene; and biobased monomers including terpenes; glycerol and glycerol derivatives obtained after reaction with at least one of epichlorohydrin, isomers of propanediol and glycolic acid; derivatives of sugars; furfural derivatives; lactic and formic acid derivatives; the monomers derived from castor oil; hydroxyalkanoic acids; bio-ethylene; bio-ethylene glycol; bio-propylene; bio-1,4-butanediol; lignin derivatives; and their mixtures.
[9" id="c-fr-0009]
9. The method of treatment according to one of claims 1 to 8, wherein the dissolved lignin recovered in the organic fluid of the washing step (2) is used in a lignin recovery process for the manufacture of a construction material or material used in aeronautics or a packaging material or a biofuel or a pharmaceutical compound or a chemical compound.
[10" id="c-fr-0010]
10. Treatment process according to one of claims 1 to 9, wherein the lignocellulosic material is softwood and 50 to 85%, preferably 50 to 75%, in% wt, of the lignin present. in the structure is dissolved during the soaking step (1).
[11" id="c-fr-0011]
11. Treatment process according to one of claims 1 to 9, wherein the lignocellulosic material is hardwood and 40 to 60%, preferably 45 to 55%, in% wt, lignin present. in the structure is dissolved during the soaking step (1).
[12" id="c-fr-0012]
12. Structure of composite material (62) comprising lignin, hemicellulose, cellulose and at least one filling compound, said structure being obtained by the implementation of the treatment method according to one of claims 1 at 11, wherein the composite material forms a three-dimensional network of transformed filler compound (59) incorporated in a structure (44 ', 45, 47, 46) of cellulose and lignin.
[13" id="c-fr-0013]
13. The material structure of claim 12, wherein the structure is substantially translucent.
[14" id="c-fr-0014]
14. Material structure according to one of claims 12 and 13, such that the structure is a finishing element, a finishing element or an element of first work.
[15" id="c-fr-0015]
15. Part comprising at least one composite material structure (62) according to one of claims 12 to 15, said part being a piece of furniture or a piece of furniture, a building element, a car part or an aeronautical part.
类似技术:
公开号 | 公开日 | 专利标题
FR3044577A1|2017-06-09|METHOD FOR PARTIAL DELIGNIFICATION AND FILLING OF A LIGNOCELLULOSIC MATERIAL, AND STRUCTURE OF COMPOSITE MATERIAL OBTAINED BY THIS PROCESS
Sandberg et al.2013|Thermo-hydro and thermo-hydro-mechanical wood processing: An opportunity for future environmentally friendly wood products
EP3237538B1|2021-09-22|Liquid |acrylic syrup, method for impregnating a fibrous substrate with said syrup, and method of manufacturing structured mechanical parts or articles using this syrup
EP3237471B1|2020-04-08|Liquid |acrylic syrup, method for impregnating a fibrous substrate with said syrup, and composite material produced after polymerisation of said impregnation syrup
CA3055904A1|2018-10-04|Transparent wood and a method for its preparation
US20200164542A1|2020-05-28|Process for supercritical or subcritical partial delignification and filling of a lignocellulosic material
Wang et al.2020|Optically transparent bamboo with high strength and low thermal conductivity
CA2511895A1|2004-08-26|Method of treating a wood element
JP2006205653A|2006-08-10|Reinforced wood impregnated with resin
Emmerich et al.2021|Growth behavior of wood-destroying fungi in chemically modified wood: wood degradation and translocation of nitrogen compounds
WO2006125797A1|2006-11-30|Method for strengthening and stabilizing a substrate made of a material comprising wood
FR2995549A1|2014-03-21|Method for treating substrate in wood material utilized for e.g. door, involves performing heat treatment for esterification of glycerol and citric acid, where material includes wood brought upto temperature between specific ranges
Frias de Albuquerque2021|Étude paramétrique d'un procédé d'imprégnation des bois feuillus
FR2909026A1|2008-05-30|Chemical stabilization of a substrate of materials comprising wood, comprises contacting the substrate with aliphatic dicarboxylic acid compound
FR2918913A1|2009-01-23|Chemical stabilization of substrate in material comprising wood, useful to maintain the outside part of wood e.g. shutters, comprises contacting the substrate with dodecanedioic acid and azelaic diacid
FR3018715A1|2015-09-25|PROCESS FOR THE TREATMENT BY DENSIFICATION OF A MATERIAL COMPRISING WOOD BY ESTERIFICATION REACTION BETWEEN SUCCINIC ACID AND GLYCEROL
CN114179182A|2022-03-15|Resin-reinforced wood-based composite material and preparation method thereof
FR2922140A1|2009-04-17|Wood substrate stabilizing method for e.g. kitchen furniture of building, involves placing substrate in contact with solution containing hydrophobic polymer precursor resin, where resin is polymerized in-situ within porosity of wood
FR3018716A1|2015-09-25|METHOD FOR THE TREATMENT BY DENSIFICATION OF A MATERIAL COMPRISING WOOD BY CHEMICAL REACTION BETWEEN CITRIC ACID AND PENTAERYTHRITOL
Salan et al.0|A PRELIMINARY STUDY ON THE DELIGNIFICATION OF THE WOOD BLOCKS VIA MICROWAVE ASSISTED ATMOSPHERIC ORGANOSOLV METHOD FOR THE PRODUCTION OF HEMICELLULOSIC SCAFFOLDS
BE624149A|
FR2922138A1|2009-04-17|Substrate i.e. wood substrate, chemical-ionic stabilizing method for e.g. staircase, of building, involves contacting substrate with salt-based compound by immersion in liquid treating bath and by solution containing water
同族专利:
公开号 | 公开日
CN113442250A|2021-09-28|
WO2017098149A1|2017-06-15|
CN108367451B|2021-08-06|
RU2747643C2|2021-05-11|
US20190077040A1|2019-03-14|
JP2019505420A|2019-02-28|
RU2018124803A3|2020-02-19|
US11254026B2|2022-02-22|
US10538012B2|2020-01-21|
EP3386697A1|2018-10-17|
FR3044577B1|2017-12-22|
BR112018011430A2|2018-11-27|
US20180370071A1|2018-12-27|
CN108367451A|2018-08-03|
CA3006341A1|2017-06-15|
RU2018124803A|2020-01-09|
EP3656520A1|2020-05-27|
WO2017098149A9|2018-05-31|
PL3386697T3|2020-06-01|
EP3386697B1|2020-01-01|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
WO1990002612A1|1988-09-16|1990-03-22|University Of South Florida|Supercritical fluid-aided treatment of porous materials|
US20100081798A1|2007-01-23|2010-04-01|Basf Se|Method for producing glucose by enzymatic hydrolysis of cellulose that is obtained from material containing ligno-cellulose using an ionic liquid that comprises a polyatomic anion|
WO2012080702A2|2010-12-15|2012-06-21|Imperial Innovations Ltd|Treatment|
WO2014113884A1|2013-01-25|2014-07-31|Ventix Environnement Inc.|Process for isolating cellulose from cellulosic biomass, isolated cellulose of type i and composite materials comprising same|
US3607355A|1967-03-06|1971-09-21|Iso Nuclear Corp|Method of making fused veneer-plastic product|
US3750303A|1971-07-09|1973-08-07|Gates T & Sons Inc|Steam tunnels for treating logs and method of treatment|
US3968276A|1972-10-25|1976-07-06|Diversified Wood Products, Inc.|Process for the preservation of wood|
CA1095663A|1975-02-12|1981-02-17|John Gordy|Pulping process|
US4239906A|1979-06-07|1980-12-16|Standard Brands Incorporated|Method for obtaining a purified cellulose product from corn hulls|
FI67241B|1981-06-10|1984-10-31|Aga Ab|SAETT FOER BLEKNING AV CELLULOSAHALTIGA MATERIAL|
CA1186855A|1982-12-09|1985-05-14|John Gordy|Semi-chemical pulping process|
JPS6162574A|1984-09-04|1986-03-31|Isao Sakata|Lignin adhesive composition|
US5169687A|1988-09-16|1992-12-08|University Of South Florida|Supercritical fluid-aided treatment of porous materials|
US5041192A|1988-09-16|1991-08-20|University Of South Florida|Supercritical delignification of wood|
PT92081A|1988-10-25|1990-04-30|Westvaco Corp|IMPROVED MULTIPLE CHLORINE LOAD BLEACHING METHOD TO REDUCE THE FORMATION OF DIOXINS AND CHLORIDE|
US4956048A|1989-04-17|1990-09-11|Westvaco Corporation|Method of alcohol washing brownstock pulp prior to a chlorination bleaching stage|
SU1657225A1|1989-07-31|1991-06-23|Уральский лесотехнический институт им.Ленинского комсомола|Method of producing catalyst for lignin extraction from wood|
FR2672296A1|1991-02-06|1992-08-07|Delorme Jean|Process for obtaining lignin-based thermoplastic compositions and products resulting therefrom|
DE19714302C2|1997-03-24|2002-01-10|Inst Getreideverarbeitung|Process for removing contaminants containing preservatives from contained or unmounted organic objects|
EP0905306A1|1997-09-26|1999-03-31|Consortium für elektrochemische Industrie GmbH|Multicomponent system for modifying, decomposing or bleaching lignin or lignin-containing materials and method of using this system|
EP1312453A3|1998-06-08|2004-06-02|Complastik Corporation|Composite articles including prepregs, preforms, laminates and sandwich moldings and methods of making the same|
JP2002536563A|1999-02-15|2002-10-29|キラムアクチボラゲット|Method for oxygen pulping lignocellulosic material and recovering pulping chemicals|
AUPQ544900A0|2000-02-04|2000-02-24|Commonwealth Scientific And Industrial Research Organisation|Treatment of cellulosic material|
US6670077B1|2000-09-29|2003-12-30|Eveready Battery Company, Inc.|Impregnated separator for electrochemical cell and method of making same|
AU1292802A|2000-11-10|2002-05-21|Sca Hygiene Prod Ab|Method of treating cellulose fibres and products obtained thereby|
JP4497782B2|2001-03-08|2010-07-07|日本製紙株式会社|Touch panel in which Newton ring is prevented and transparent electrode for the touch panel|
US6649245B2|2001-03-30|2003-11-18|Thomas A. Lenderink|Flexible real wood composition veneer|
FR2838369B1|2002-04-10|2004-07-02|Lapeyre|PROCESS FOR THE TREATMENT OF LIGNOCELLULOSIC MATERIAL, IN PARTICULAR WOOD AND A MATERIAL OBTAINED BY THIS PROCESS|
US20040090426A1|2002-11-07|2004-05-13|Eastman Kodak Company|Transparent flexible sheet for resistive touch screen|
CN1201909C|2003-01-24|2005-05-18|南通纺织职业技术学院|Wood decorative material biological enzyme pretreatment method|
JP2005156859A|2003-11-25|2005-06-16|Tohoku Pioneer Corp|Driving device and driving method of self-luminous display panel|
US20050233069A1|2003-11-25|2005-10-20|Dai Nippon Printing Co., Ltd.|Antiglare film|
EP1776176B1|2004-08-13|2015-09-16|McMASTER UNIVERSITY|Process for preparing a filtration membrane comprising a non-crosslinked gel polymer|
CN1813900B|2005-02-05|2010-11-10|南京海陵中药制药工艺技术研究有限公司|Kadsura longipedunculata lignin extract and its preparing method and use|
CA2606781A1|2005-05-02|2006-11-09|Basf Aktiengesellschaft|Method for impregnating lignocellulosic materials with effect agents|
US7633583B2|2005-05-23|2009-12-15|Ran-Hong Raymond Wang|Controlling polarization for liquid crystal displays|
CN1872508A|2005-05-30|2006-12-06|宋建国|Hardening treatment for timber|
ITTO20050569A1|2005-08-09|2007-02-10|St Microelectronics Srl|DEVICE AND METHOD OF DETERMINING THE CONTACT POSITION AND CONTACT SENSITIVE ELECTRONIC DEVICE|
US20120105370A1|2005-12-12|2012-05-03|Nupix, LLC|Electroded Sheet for a Multitude of Products|
AT468952T|2006-07-20|2010-06-15|Yamaha Corp|METHOD FOR PRODUCING A WOODEN WOOD, WOODEN STRUCTURE, INTERIOR MATERIAL OF A VEHICLE AND ACOUSTIC STRUCTURE PROCESSED BY THIS METHOD|
CN1911612A|2006-08-25|2007-02-14|南京林业大学|Method of lignin modification for veneer|
CN1985891B|2006-12-15|2011-04-27|吉林省泉阳林业局|Compound Chinese medicine preparation with liver protecting function and its preparing process|
WO2008098036A1|2007-02-06|2008-08-14|North Carolina State University|Product preparation and recovery from thermolysis of lignocellulosics in ionic liquids|
WO2008112291A2|2007-03-14|2008-09-18|The University Of Toledo|Biomass pretreatment|
JP4388966B2|2007-03-16|2009-12-24|富士通株式会社|Coordinate input device|
US9628880B2|2008-04-07|2017-04-18|Koss Corporation|Wooden or other dielectric capacitive touch interface and loudspeaker having same|
CN101279458A|2008-05-15|2008-10-08|华南理工大学|Inorganic composite plate and preparation and use thereof|
JP5339341B2|2008-08-13|2013-11-13|宜章 大木|Separation method of wood fibers as fiber solids by subcritical state|
JP2010163497A|2009-01-13|2010-07-29|Toshiba Corp|Polymer composition material and method for producing the same|
CN101476252B|2009-01-21|2011-09-28|任宪君|Method for extracting cellulose, lignose and compound fertilizer from cotton-seed hull|
GB0901910D0|2009-02-06|2009-03-11|Kurawood Plc|Chemical modification of lignocellulosic material|
US8772406B2|2009-08-06|2014-07-08|Robert J. Linhardt|Synthetic wood composite|
CN101649125B|2009-09-15|2011-06-29|福州大学|Lignin modified high molecular compatible additive and preparation method thereof|
IN2014DN08895A|2012-05-31|2015-05-22|Nalco Co|
TWI511019B|2009-11-17|2015-12-01|Wistron Corp|Flat-surface resistive touch panel|
KR100977721B1|2010-01-25|2010-08-24|주식회사 남보|Biomass pretreatment method using cyclic lignin extraction reactor system and ammonia|
US8366877B2|2010-03-10|2013-02-05|Nalco Company|Lipohydrophilic glycerol based polymers as digestion aids for improving wood pulping processes|
JP5735833B2|2010-03-31|2015-06-17|大阪瓦斯株式会社|Method for producing cellulose|
TWI408583B|2010-04-19|2013-09-11|Wistron Corp|Slim type touch device|
JP2012009233A|2010-06-23|2012-01-12|Toshiba Corp|Insulating structure material and production method for the same|
US8575374B1|2010-10-21|2013-11-05|Hugh C. DeLong|Ionic liquids processing of biomass to reducing sugars and other dehydration products|
KR101230191B1|2010-12-14|2013-02-06|삼성디스플레이 주식회사|Touch Screen Panel and Fabricating Method for the Same|
JP5589871B2|2011-01-27|2014-09-17|トヨタ自動車株式会社|Method for treating cellulosic biomass, method for producing sugar, alcohol or organic acid from cellulosic biomass|
CN102152356B|2011-03-23|2014-01-15|中国林业科学研究院木材工业研究所|Method for preparing densified woods through silica sol|
JP2012226276A|2011-04-22|2012-11-15|Fujifilm Corp|Cellulose acylate film, polarizing plate and liquid crystal display device|
CN102785274A|2011-05-17|2012-11-21|南京林业大学|Pretreatment method used before processing fast growing wood surface concave-convex textures|
US20130167603A1|2011-07-03|2013-07-04|Christopher Francis Bathurst|Methods and systems for processing plants and converting cellulosic residue to crude bio-oils|
US9158143B2|2011-09-12|2015-10-13|Apple Inc.|Dual purpose touch sensor panel and optical retarder|
CN104136579A|2011-11-03|2014-11-05|索拉瑞控股有限公司|Method for removal of toxic waste from timber|
GB2499242A|2012-02-10|2013-08-14|Alterix Ltd|methods of operating excitation circuitry and/or measurement circuitry in a digitiser and a method of manufacturing a transducer for a digitiser|
EP2850109B1|2012-05-14|2017-08-16|Metsä Fibre Oy|Method of separation of hemicellulose and cellulose from polysaccharide sources|
CN102704297B|2012-05-29|2014-10-29|南京林业大学|Method for separating non-wood lignocellulosic biomass lignin with composite solvents|
WO2014002674A1|2012-06-26|2014-01-03|国立大学法人鳥取大学|Method for producing lignin from biomass using lignin-dissolving ionic liquid, and method for producing lignin, hemicellulose and cellulose|
KR102028169B1|2012-07-31|2019-10-02|삼성에스디아이 주식회사|Electrode having 3-dimensional pore network structure, lithium battery including the electrode, and method for manufacturing the electrode|
US20140048221A1|2012-08-20|2014-02-20|Celanese International Corporation|Methods for extracting hemicellulose from a cellulosic material|
CN102864672B|2012-09-17|2015-06-24|北京林业大学|Method for extracting lignin|
CN202882247U|2012-11-05|2013-04-17|左大刚|Archaized mechanism|
SE537712C2|2012-11-13|2015-10-06|Stora Enso Oyj|Thermally reactive thermoplastic intermediate comprising conifers lignin and process for the preparation thereof.|
KR102003371B1|2012-11-16|2019-10-01|삼성전자주식회사|Apparatas and method for adjusting of screen brightness in an electronic device|
NL2010006C2|2012-12-18|2014-06-19|Stichting Energie|Process for enzymatic hydrolysis of cellulose.|
KR20140086584A|2012-12-28|2014-07-08|삼성전기주식회사|Photo-sensitive resin composition for bezel of touch screen module and bezel for touch screen module using the same|
JP6206089B2|2013-04-23|2017-10-04|Jnc株式会社|Polysaccharide monolith structure and production method thereof|
JP2015020307A|2013-07-17|2015-02-02|大建工業株式会社|Intermediate material of woody decorative plate and woody decorative plate|
JPWO2015033701A1|2013-09-05|2017-03-02|コニカミノルタ株式会社|Antifogging film, antifogging glass, glass laminate and liquid crystal display device|
JP2015055796A|2013-09-12|2015-03-23|富士フイルム株式会社|Optical film and display device|
JP6244808B2|2013-10-17|2017-12-13|ヤマハ株式会社|Composite material for acoustic material and method for producing composite material for acoustic material|
US20160010279A1|2013-12-06|2016-01-14|University Of Maryland At College Park|Scalable, highly transparent paper with microsized fiber|
CN103993042B|2014-01-07|2016-08-24|天津科技大学|A kind of lignocellulose material co-producing bio ethanol and the method for pulullan|
WO2015160908A1|2014-04-15|2015-10-22|Celgard, Llc|Electrically conductive, transparent, translucent, and/or reflective materials|
KR102248460B1|2014-08-08|2021-05-07|삼성디스플레이 주식회사|Touch screen panel and fabrication method of the same|
CN104389216B|2014-10-21|2016-05-25|国际竹藤中心|The method of separating lignin and holocellulose and application from lignocellulose raw material|
CN104448585A|2014-11-28|2015-03-25|青岛科技大学|Technology for processing ethylene propylene diene monomer rubber/polypropylene/lignin composite material|
CN104651964A|2015-01-28|2015-05-27|南通联海维景生物有限公司|Preparation method of cellulose nanofiber|
DK3266223T3|2015-03-04|2019-08-12|Bang & Olufsen As|Panel with two-handed user interface for a multi-room media player|
FI127740B|2015-05-29|2019-01-15|Upm Kymmene Corp|A method and an apparatus for forming a lignin fraction, a lignin composition and its use|
DE102015113522A1|2015-08-17|2017-02-23|Universität Stuttgart|Porous monolithic hybrid reactor, a process for its preparation and its use|
FR3044577B1|2015-12-07|2017-12-22|Timothee Boitouzet|METHOD FOR PARTIAL DELIGNIFICATION AND FILLING OF A LIGNOCELLULOSIC MATERIAL, AND STRUCTURE OF COMPOSITE MATERIAL OBTAINED BY THIS PROCESS|
EP3411449A4|2016-02-04|2019-10-09|University of Maryland, College Park|Transparent wood composite, systems and method of fabrication|
US20190113791A1|2016-02-09|2019-04-18|Dai Nippon Printing Co., Ltd.|Optical laminate and production method therefor, front panel, and image display device|
US20180016355A1|2016-07-14|2018-01-18|Api Intellectual Property Holdings, Llc|Solvent-based processes for producing nanocellulose, and compositions and products produced therefrom|
CN106243391B|2016-08-05|2018-12-11|南京林业大学|The preparation method of transparent timber|
CN106493827B|2016-10-12|2018-07-20|浙江农林大学|A kind of engineered wood and preparation method thereof|
CN108250677A|2016-12-29|2018-07-06|中国科学院深圳先进技术研究院|A kind of polymer matrix composite comprising filler grain three-dimensional network and preparation method thereof|
FR3061908B1|2017-01-13|2019-05-31|Centre National De La Recherche Scientifique|PROCESS FOR TREATING BIOMASS|
CN110603124B|2017-03-29|2022-03-04|切卢特克股份公司|Transparent wood and preparation method thereof|
EP3609661A4|2017-04-10|2020-11-18|University of Maryland, College Park|Strong and tough structural wood materials, and methods for fabricating and use thereof|
JPWO2018211945A1|2017-05-18|2020-05-28|株式会社ダイセル|Carbon dioxide separation membrane and manufacturing method thereof|
US10411222B2|2017-05-23|2019-09-10|University Of Maryland, College Park|Transparent hybrid substrates, devices employing such substrates, and methods for fabrication and use thereof|
FR3067275A1|2017-06-07|2018-12-14|Timothee Boitouzet|PROCESS FOR SUPERCRITICALLY OR SUBCRITICALLY PARTIALLY DELIGNIFYING AND FILLING A LIGNOCELLULOSIC MATERIAL|
EP3681682A4|2017-09-15|2021-06-16|University of Maryland, College Park|Delignified wood materials, and methods for fabricating and use thereof|
FR3077895B1|2018-02-09|2020-02-28|Sas Woodoo|TACTILE DETECTION DEVICE WITH TACTILE INTERFACE IN COMPOSITE MATERIAL|
FR3086196A1|2018-09-20|2020-03-27|Sas Woodoo|PART IN LIGNOCELLULOSIC MATERIAL AND METHOD FOR MANUFACTURING SUCH A PART|FR3044577B1|2015-12-07|2017-12-22|Timothee Boitouzet|METHOD FOR PARTIAL DELIGNIFICATION AND FILLING OF A LIGNOCELLULOSIC MATERIAL, AND STRUCTURE OF COMPOSITE MATERIAL OBTAINED BY THIS PROCESS|
EP3411449A4|2016-02-04|2019-10-09|University of Maryland, College Park|Transparent wood composite, systems and method of fabrication|
CN110603124B|2017-03-29|2022-03-04|切卢特克股份公司|Transparent wood and preparation method thereof|
US10411222B2|2017-05-23|2019-09-10|University Of Maryland, College Park|Transparent hybrid substrates, devices employing such substrates, and methods for fabrication and use thereof|
FR3067275A1|2017-06-07|2018-12-14|Timothee Boitouzet|PROCESS FOR SUPERCRITICALLY OR SUBCRITICALLY PARTIALLY DELIGNIFYING AND FILLING A LIGNOCELLULOSIC MATERIAL|
EP3684571A4|2017-09-08|2021-07-14|DTE Materials Incorporated|Selectively depolymerizing cellulosic materials for use as thermal and acoustic insulators|
FR3077895B1|2018-02-09|2020-02-28|Sas Woodoo|TACTILE DETECTION DEVICE WITH TACTILE INTERFACE IN COMPOSITE MATERIAL|
CN108456401B|2018-05-02|2021-04-23|北京中环鑫汇科技有限公司|Pipeline composite material and preparation method thereof|
FR3086196A1|2018-09-20|2020-03-27|Sas Woodoo|PART IN LIGNOCELLULOSIC MATERIAL AND METHOD FOR MANUFACTURING SUCH A PART|
CN109129798B|2018-10-30|2021-06-22|北京英华高科技有限公司|High-performance structural material and preparation method thereof|
CN109366637B|2018-11-23|2021-04-16|浙江农林大学|Bamboo veneer, bamboo veneer plywood and preparation method thereof|
CN109531743B|2018-11-28|2020-09-29|浙江农林大学|Bamboo veneer, PVC composite floor and preparation method thereof|
RU2712521C1|2019-02-07|2020-01-29|Общество с ограниченной ответственностью "Модификация"|Method of producing modified wood|
CN110328727A|2019-05-09|2019-10-15|浙江景兴纸业股份有限公司|A kind of transparent timber and the application of the method and its preparation preparing transparent timber using organic solvent|
TWI708797B|2019-07-17|2020-11-01|元智大學|Method for preparing photopolymerized polyglyceryl sebacate copolymerized lignin elastomer|
TWI708791B|2019-07-17|2020-11-01|元智大學|Manufacturing method of photopolymerized elastomer|
CN111109859A|2019-12-20|2020-05-08|肇庆市现代筑美家居有限公司|Practice thrift extensible formula dining table in space|
FR3112449A1|2020-07-08|2022-01-14|Sas Woodoo|Method for manufacturing an electrically conductive device in lignocellulosic material|
CN112171830A|2020-09-15|2021-01-05|南京大学|High-strength wood and preparation method thereof|
CN112895048A|2021-01-18|2021-06-04|浙江农林大学|Method for recycling mildewed dried bean curd stick wood|
法律状态:
2016-11-25| PLFP| Fee payment|Year of fee payment: 2 |
2017-06-09| PLSC| Publication of the preliminary search report|Effective date: 20170609 |
2017-10-20| PLFP| Fee payment|Year of fee payment: 3 |
2018-10-26| PLFP| Fee payment|Year of fee payment: 4 |
2019-10-11| PLFP| Fee payment|Year of fee payment: 5 |
2020-10-21| PLFP| Fee payment|Year of fee payment: 6 |
2021-03-05| TP| Transmission of property|Owner name: SAS WOODOO, FR Effective date: 20210122 |
优先权:
申请号 | 申请日 | 专利标题
FR1561953A|FR3044577B1|2015-12-07|2015-12-07|METHOD FOR PARTIAL DELIGNIFICATION AND FILLING OF A LIGNOCELLULOSIC MATERIAL, AND STRUCTURE OF COMPOSITE MATERIAL OBTAINED BY THIS PROCESS|FR1561953A| FR3044577B1|2015-12-07|2015-12-07|METHOD FOR PARTIAL DELIGNIFICATION AND FILLING OF A LIGNOCELLULOSIC MATERIAL, AND STRUCTURE OF COMPOSITE MATERIAL OBTAINED BY THIS PROCESS|
RU2018124803A| RU2747643C2|2015-12-07|2016-12-07|Process for partial removal of lignin and filling of lignocellulosic material, and structure of composite material produced by this process|
EP19219690.5A| EP3656520A1|2015-12-07|2016-12-07|Method for partial delignification and filling of a lignocellulosic material, and composite material structure that can be obtained by said method|
PCT/FR2016/053247| WO2017098149A1|2015-12-07|2016-12-07|Process for partial delignification and filling of a lignocellulosic material, and composite structure able to be obtained by this process|
US15/781,978| US11254026B2|2015-12-07|2016-12-07|Process for partial delignification and filling of a lignocellulosic material, and composite material structure able to be obtained by this process|
BR112018011430-8A| BR112018011430A2|2015-12-07|2016-12-07|process of partial delignification and filling of a lignocellulosic material, and structure of composite material that can be obtained by this process|
CN201680072162.3A| CN108367451B|2015-12-07|2016-12-07|Method for partial delignification and filling of lignocellulosic material and composite structure obtainable by such a method|
CA3006341A| CA3006341A1|2015-12-07|2016-12-07|Process for partial delignification and filling of a lignocellulosic material, and composite structure able to be obtained by this process|
JP2018548290A| JP2019505420A|2015-12-07|2016-12-07|Method for partial delignification and filling of lignocellulosic material, and composite material structure obtained by the method|
EP16813100.1A| EP3386697B1|2015-12-07|2016-12-07|Process for partial delignification and filling of a lignocellulosic material, and composite structure able to be obtained by this process|
PL16813100T| PL3386697T3|2015-12-07|2016-12-07|Process for partial delignification and filling of a lignocellulosic material, and composite structure able to be obtained by this process|
CN202110803481.XA| CN113442250A|2015-12-07|2016-12-07|Method for partial delignification and filling of lignocellulosic material and composite structure obtainable by such a method|
US16/185,342| US10538012B2|2015-12-07|2018-11-09|Process for partial delignification and filling of a lignocellulosic material, and composite material structure able to be obtained by this process|