专利摘要:
The subject of the invention is a sheet for a stamped part of a lining or bodywork structure, also known as a white body, made of aluminum alloy of composition (% by weight): Si: 0.85 - 1.20 Fe: <0 , Cu: 0.10 - 0.30 Mg: 0.70 - 0.90 Mn: <0.30 Zn: 1.10 - 1.60 V: 0.05 - 0.30 Ti: 0.05 - 0.20 other elements <0.05 each and <0.15 in total, remaining aluminum, having after dissolution, quenching, pre-tempering or reversion, optionally maturing at room temperature of between 72 hours and 6 months, controlled tension deformation of 2% and paint baking treatment of 20 min at 185 ° C, a yield strength Rp0.2 of at least 300 MPa. The sheets according to the invention make it possible to reduce the thickness of the pieces while satisfying all the other properties required.
公开号:FR3036986A1
申请号:FR1555129
申请日:2015-06-05
公开日:2016-12-09
发明作者:Estelle Muller;Mary-Anne Kulas;Olivier Rebuffet
申请人:Constellium Neuf Brisach SAS;
IPC主号:
专利说明:

[0001] FIELD OF THE INVENTION The invention relates to the field of Al-Si-Mg alloy sheets, more particularly to alloy type AA6xxx according to the designation of the "Aluminum Association", added with hardening elements and intended for the manufacture by stamping of lining parts, structure or reinforcement of the white box of motor vehicles. STATE OF THE ART In the preamble, all the aluminum alloys referred to below are designated, unless otherwise indicated, according to the designations defined by the "Aluminum Association" in the "Registration Record Series" that it publishes. regularly. All indications regarding the chemical composition of the alloys are expressed as a percentage by weight based on the total weight of the alloy. The definitions of the metallurgical states are given in the European standard EN 515. The static mechanical characteristics in tension, in other words the tensile strength Rm, the conventional yield strength at 0.2% elongation Rp0,2 , and elongation at break A%, are determined by a tensile test according to standard NF EN ISO 6892-1. Aluminum alloys are increasingly used in the construction of motor vehicles because their use reduces the weight of vehicles and thus reduce fuel consumption and greenhouse gas emissions. The aluminum alloy sheets are used in particular for the manufacture of many parts of the "white box" among which we distinguish: body skin parts (or outer body panels) as the front wings, 3036986 2 the roof or roof, bonnet, boot or door skin; lining parts such as door, wing, tailgate or hood liners; and finally the structural parts, such as the longitudinal members, the aprons, the load floors and the front, middle and rear feet.
[0002] If many pieces of skin and lining are already made of aluminum alloy sheets, the transposition of steel to aluminum for reinforcing or structural parts, having higher characteristics, proves more difficult due to the fact that aluminum alloys are less formable than steels in the first instance and, in a second step, mechanical characteristics are generally lower than those of the steels used for this type of part. Indeed, for reinforcing or structural type applications, a set of properties, sometimes antagonistic, is required such as: a high formability in the delivery state, state T4, in particular for stamping operations, a limit of controlled elasticity in the state of delivery of the sheet to control the elastic return during the shaping, a high mechanical resistance after cataphoresis and baking of the paints to obtain a good mechanical resistance in service while minimizing the weight of the part , Good shock absorption capacity for application to bodywork parts, good behavior in the various assembly methods used in automotive bodywork such as spot welding, laser welding bonding, clinching or riveting, good corrosion resistance, especially intergranular corrosion, stress corrosion and corrosion Filiform ion of the finished part, compatibility with the requirements of the recycling of manufacturing waste or recycled vehicles, an acceptable cost for mass production. There are already, however, mass-produced motor vehicles with a white box consisting mainly of aluminum alloys. For example the model Ford F-150 version 2014 consists of the alloy structure AA6111.
[0003] 3036986 3 This alloy was developed by the group "Alcan" in the years 1980-1990. Two references describe this development work: PE Fortin et al, "An optimized Al alloy for Auto body sheet applications", SAE technical conference, March 1984 describes the following composition: [Fortin] Si Cu Fe Mn Mg Cr Zn Ti AA6111 0, 85 0.20 0.75 0.20 0.72 - - - MJ Bull et al, "Al sheet alloys for structural and skin applications", 25th ISATA symposium, Paper 920669, June 1992: The main property remains a strong mechanical strength , although it is initially intended to resist indentation for skin-type applications: "A yield-strength of 280 MPa is achieved after 2% pre-strain and 30 min at 177 ° C".
[0004] On the other hand, other alloys of the AA6xxx family with high mechanical properties have been developed for aeronautical or automotive applications. Thus, the alloy AA6056 type, whose development dates back to the 1980s at "Pechiney" has been the subject of many works and many publications, either 20 to optimize the mechanical characteristics, or to improve the resistance to intergranular corrosion . We will retain the automotive application of this type of alloy, which was the subject of a patent application (WO2004113579A1). Alloys of the type AA6013 have also been the subject of much work.
[0005] For example, in "Alcoa", in US2002039664 published in 2002, an alloy comprising 0.6-1.15% Si; 0.6-1% Cu; 0.8-1.2% Mg; 0.55-0.86% Zn; less than 0.1% Mn, 0.2-0.3% Cr and about 0.2% Fe, used in the T6 state, combines good resistance to intergranular corrosion, as well as a Rpo, 2 of 380 MPa. At "Aleris", an application published in 2003, W003006697, relates to an alloy of the AA6xxx series with 0.2 to 0.45% Cu. The object of the invention is to provide an alloy of the AA6013 type with a reduced Cu level, targeting 355 MPa of Rm at the T6 state and good resistance to intergranular corrosion. The composition claimed is as follows: 0.8-1.3% Si, 0.2-0.45% Cu, 0.5-1.1% Mn, 0.45-1.0% Mg.
[0006] Finally, it should be noted that in all the aforementioned examples, obtaining high mechanical properties (Rpo, 2, Rm) is achieved by using alloys containing at least 0.5% copper.
[0007] Problem The object of the present invention is to provide aluminum alloy sheets for lining, reinforcement or automobile body structure having mechanical strength in service, after shaping and baking of the paints, also or even higher. , that the sheets of the prior art, while having a good resistance to corrosion, in particular intergranular or filiform, a formability by stamping at satisfactory ambient temperature and good behavior in various assembly methods such as welding by points, laser welding, gluing, clinching or riveting.
[0008] OBJECT OF THE INVENTION The object of the invention is a sheet for a stamped part of a lining, reinforcement or automobile bodywork structure, also known as a white box, made of aluminum alloy of the AA6xxx series, having a Cu content. low, added with hardening elements including Zn, V and Ti, typically of thickness between 1 and 5 mm, and composition (% by weight): Si: 0.85 - 1.20 and preferably: 0 , 90 - 1.10 Fe: <0.30 and preferably: 0.15 - 0.25 Cu: 0.10 - 0.30 and preferably: 0.10 - 0.20 Mg: 0.70 - 0 , 90 and preferably: 0.70 - 0.80 Mn: <0.30 and preferably: 0.10 - 0.20 3036986 Zn: 1.10 - 1.60 and preferably: 1.20 - 1.50 V: 0.05 - 0.30 and preferably: 0.10 - 0.20 Ti: 0.05 - 0.20 and preferably: 0.08 - 0.15 other elements <0.05 each and <0 A total of 15 remains aluminum. It also relates to a method of manufacturing said sheets as above, comprising the steps s following: - the typical vertical semi-continuous casting of a plate and its possible scalping, - the homogenization at a temperature of 550 to 570 ° C with a maintenance between 2 and 12 h, preferably between 4 and 6 h, followed by rapid cooling to ambient temperature, typically with forced air or with water, - reheating at a temperature of between 450 and 550 ° C. with a hold of between 30 minutes and 3 hours, preferably substantially 2 h, 15 - the hot rolling of the plate in a strip of thickness between 3 and 10 mm, - the cold rolling to the final thickness typically between 1 and 5 mm, - the dissolution in solution of the rolled strip at a temperature above the solvus temperature of the alloy, while avoiding burn, ie between 550 and 570 ° C for 30 seconds to 5 minutes, followed by quenching at a rate of more than 50 ° C / s and better still at least 100 ° C / s, - the pre-income, or reversion, by winding at a temperature at least 60 ° C followed by cooling in the open air of the coil obtained.
[0009] According to another variant, the homogenization and reheating steps above are replaced by a single reheating step at a temperature between 550 and 570 ° C with a maintenance between 2 and 12 h, preferably between 4 and 6 h followed by hot rolling as above.
[0010] According to an advantageous embodiment, the sheet obtained by the above process has, after optional maturation at room temperature of between 72 h and 6 months, a controlled tensile pre-deformation of 2% to simulate shaping, and treatment. For example, for a period of about 20 minutes at 185 ° C., a yield strength of Rpo 2 of at least 300 MPa. Equally advantageously, the sheet obtained by the aforementioned process, in the metallurgical state T6 according to the European standard EN 515, is typically after a complementary heat treatment at 205 ° C. for 2 hours or equivalent, a yield strength Rpo , 2 of at least 350 MPa. Also advantageously, the sheet obtained by the aforementioned method has a good resistance to corrosion, especially intergranular and filiform. Finally, such a sheet in a thickness of 2 mm, obtained by the aforementioned method, after optional maturation at ambient temperature of between 72 h and 6 months, a controlled tensile pre-deformation of 10%, and baking treatment of the paints, Typically for 20 min at 185 ° C, has a "three point bend angle" aio%, measured according to NF EN ISO 7438 and VDA procedure 238-100, of at least 60 °.
[0011] DESCRIPTION OF THE FIGURES FIG. 1 shows the device for "three-point folding test" consisting of two rollers R, a punch B of radius r for folding the sheet T of thickness t.
[0012] FIG. 2 shows the sheet T after the "three-point folding" test with the internal angle 13 and the external angle, the measured result of the test: again called a%. Figure 3 shows the dimensions in mm of the tools used to determine the parameter value known to those skilled in the art as LDH (Limit Dome Height) characteristic of the drawability of the material.
[0013] The invention is based on the Applicant's finding that a narrow composition range within the composition of an alloy of the AA6xxx family registered at the Aluminum Association, associated with a combined addition of Zn, V and Ti, allowed to obtain all the desired properties, namely high mechanical strength after shaping and baking paints, related in particular to the addition of zinc but combined surprisingly and unexpectedly, due in principle to the simultaneous presence of V and Ti, a very satisfactory resistance to corrosion, intergranular and filiform, and a formability in stamping at satisfactory ambient temperature. The concentration ranges imposed on the constituent elements of this type of alloy are therefore explained by the following reasons: Si: The mechanical properties of the aluminum alloys increase regularly with the silicon content. Silicon is, along with magnesium, the second alloying element of aluminum-magnesium-silicon systems (family AA6xxx) to form the intermetallic compounds Mg2Si or Mg5Si6 which contribute to the structural hardening of these alloys. The presence of silicon, at a content of between 0.85% and 1.20%, combined with the presence of magnesium at a content of between 0.70% and 0.90% makes it possible to obtain the Si / Mg ratio. required to achieve the desired mechanical properties while ensuring good corrosion resistance and stamping shaping at satisfactory ambient temperature. The range of the most advantageous content is from 0.90 to 1.10%. Mg: The level of mechanical characteristics of the alloys of the AA6xxx family is proportional to the magnesium content. Combined with silicon to form the Mg2Si or Mg5Si6 intermetallic compounds, magnesium contributes to the increase in mechanical properties. A minimum content of 0.70% is necessary to obtain the required level of mechanical characteristics and to form sufficient hardening precipitates. In addition, the solvus temperature, corresponding to the dissolution temperature, of these alloys is very dependent on the magnesium content. Beyond 0.90%, the solvus temperature becomes too high thus posing problems of industrial solution. The range of the most advantageous content is 0.70 to 0.80%.
[0014] 5 Fe: It is always present as impurity in "primary aluminum", since it comes, like silicon, ore, bauxite, whose alumina is extracted. A minimum content of 0.05%, and better still 0.15%, substantially decreases the solubility of manganese in solid solution, which makes it possible to obtain a sensitivity at the rate of positive deformation, delays the rupture during the deformation after necking, and thus improves ductility and formability. Iron is also necessary for the formation of a high density of intermetallic particles guaranteeing good "hardenability" during shaping. In these grades iron also makes it possible to control the size of the grains. Above a content of 0.30%, too many intermetallic particles are created with a detrimental effect on ductility and corrosion resistance. The most preferred range is 0.15 to 0.25%. Mn: its content is limited to 0.30%. An addition of manganese above 0.05% can increase the mechanical characteristics by solid solution effect, but beyond 0.3%, it would very strongly decrease the sensitivity to the deformation rate and therefore the ductility. . An advantageous range is from 0.10 to 0.20%.
[0015] Cu: In alloys of the AA6000 family, copper is an effective hardening element in participating in the hardening precipitation. At a minimum content of 0.10%, its presence makes it possible to obtain higher mechanical characteristics. Above 0.30% copper has a negative influence on the corrosion resistance.
[0016] The most preferred range of content is from 0.10 to 0.20%. Zn: the effect of Zn addition in AA6xxx on mechanical properties and corrosion resistance is not fully understood. A minimum content of 1.10% is required to achieve the required level of mechanical characteristics by solid solution hardening. In addition, the addition of Zn in aluminum alloys of the AA6xxx family modifies the temperature of the solidus. The more Zn is added, the lower the solidus temperature, thus reducing the difference between solvus and solidus temperature and making it difficult to industrialize such an alloy. Beyond 1.60%, this difference becomes too critical. The best value range is 1.20 to 1.50%. V and Ti: A minimum content of 0.05% of each of these elements is necessary to obtain a solid solution hardening leading to the required mechanical characteristics and, combined with the addition of Zn, each of these elements has plus a favorable effect on the ductility in service and the resistance to corrosion. On the other hand, a maximum content of 0.20% for Ti and 0.30% for V is required not to form primary phases during vertical casting, which have a detrimental effect on all of the claimed properties. The most advantageous range of content is 0.10 to 0.20% for V and 0.08 to 0.15 for Ti. The method of manufacturing the sheets according to the invention typically comprises the casting of a plate, possibly the scalping of this plate, followed by: homogenization at a speed of at least 30 ° C./h up to a temperature from 550 to 570 ° C with a hold between 2 and 12 h, preferably between 4 and 6 h, followed by rapid cooling with forced air or water to the ambient, then reheating to a temperature between 450 and 550 ° C with a maintenance between 30 min and 3 h, preferably substantially 2 h, 25 is directly heating at a temperature of 550 to 570 ° C with a maintenance between 2 and 12 h, preferably between 4 and 6 h. Then comes the hot rolling of the plate in a strip of thickness between 3 and 10 mm, the cold rolling to the final thickness typically between 1 and 5 mm, the dissolution of the strip laminated to a temperature above the solvus temperature of the alloy, while avoiding burn, ie between 550 and 570 ° C for 30 s to 5 min, quenching at a speed of more than 50 ° C / s and preferably at least 100 ° C / s, and finally the pre-income, or reversion, by winding at a temperature of at least 60 ° C followed by cooling in the open air of the coil obtained. Thus, the sheets according to the invention have a satisfactory ability to draw at room temperature. Just as advantageously, they have, in use, after shaping, assembly and baking paints, high mechanical properties, good resistance to corrosion, in particular intergranular corrosion and filiform corrosion.
[0017] Examples Preamble Table 1 summarizes the nominal chemical compositions (% by weight) of the alloys used in the tests. The foundry plates of these different alloys were obtained by vertical semicontinuous casting. After scalping, these different plates have undergone a homogenizing and / or reheating heat treatment whose temperatures are given in Table 2. The plates of cases 1, 6, 7, 8 and 10 have undergone a homogenization treatment. at 570 ° C consisting of a rise in temperature at a rate of 30 ° C / h to 570 ° C, a maintenance of about 5 hours at 570 ° C and a controlled cooling with forced air until at room temperature. This homogenization step is followed by a heating step consisting of a rise in temperature at a rate of 70 ° C./h up to 480 ° C. with a maintenance time of the order of 40 minutes, directly monitored. hot rolling. The plates of case 2 have undergone a homogenization treatment at 562 ° C. consisting of a temperature rise at a rate of 30 ° C./h up to 562 ° C., a maintenance of the order of 5 hours at 562 ° C. ° C then controlled cooling to room temperature. The homogenization step is followed by a heating step consisting of a rise in temperature at a speed of 60 ° C./h up to 530 ° C. with a maximum temperature retention of 2 hours, followed by rolling. hot. The plates of cases 3 and 5 were heated up to 565 ° C and 550 ° C, respectively, with a minimum hold of 2 hours at these temperatures, followed directly by hot rolling. The plates of cases 4 and 9, made of AA6016 and AA5182 type alloys, have undergone standard homogenizations for these types of alloys.
[0018] The next hot rolling step is carried out on a reversible rolling mill followed, according to the case, by a hot tandem rolling mill with 4 stands up to a thickness of between 3 and 10 mm. The hot rolling output thicknesses of the tested cases are given in Table 2. This hot rolling step is followed by a cold rolling step which makes it possible to obtain sheets of thickness between 1.7 and 2.5. mm. The cold rolling output thicknesses of the tested cases are given in Table 2. The rolling steps are followed by a solution heat treatment and quenching step. The dissolution is done at a temperature above the solvus temperature of the alloy, while avoiding burning. The solution sheet is then quenched at a minimum rate of 50 ° C / sec. For all cases, except for cases 4 and 9, this step is carried out in a passing furnace by raising the temperature of the metal to 570 ° C in less than about one minute directly followed by quenching. For case 4, alloy AA6016 type, the cold rolling was also followed by a heat treatment at the end of the range and consists in a dissolution and quenching carried out in a passing oven by raising the temperature of the metal up to 540 ° C in about 30 seconds and quenching at a minimum speed of 50 ° C / sec. For case 9, of AA5182 type alloy, the recrystallization annealing took place in a pass-through furnace and consisted in bringing the metal to a temperature of 365 ° C. in approximately 30 seconds and then cooling it.
[0019] The quenching is followed by a pre-tempered heat treatment, intended to improve the curing performance during the baking of the paints. For all the cases tested, except case 9, this step is performed by winding at a temperature of at least 60 ° C followed by cooling in the open air. The winding temperatures are described in Table 2.
[0020] 3036986 12 Composition Si Fe Cu Mn Mg Zn Ti V Invention 1 0.92 0.19 0.16 0.18 0.72 1.47 0.08 0.15 Invention 2 0.94 0.20 0.17 0.17 0.72 1.52 0.11 0.15 Invention 3 0.95 0.10 0.18 0.74 1.20 0.10 0.14 Alloy 4 1.05 0.25 0.09 0.17 0.37 0.02 0.02 0.00 Alloy 5 1.08 0.25 0.18 0.18 0.57 0.01 0.02 0.00 Alloy 6 0.81 0.15 0.16 0.17 0.79 0.01 0.02 0.00 Alloy 7 0.63 0.19 0.16 0.17 0.97 1.46 0.09 0.15 Alloy 8 0.93 0.20 0.16 0.18 0.78 0.05 0.03 0.01 Alloy 9 <0.20 <0.35 0.07 0.33 4.65 0.01 0.02 0.00 Alloy 10 0.79 0.29 0.80 0.003 0.71 0.49 0.05 0.01 Table 1 Homogenization Reheating Thickness Thickness Pre-revenue output LAF output LAF Invention 1 570 ° C 480 ° C 10 mm 2.0 mm 85 ° C Invention 2 562 ° C 530 ° C 10 mm 2.5 mm 65 ° C Invention 3 X 565 ° C 10 mm 2.0 mm 80 ° C Alloy 4 6.0 mm 2.0 mm 70 ° C Alloy 5 X 550 ° C 3.0 mm 1.7 mm 60 ° C Alloy 6 570 ° C 480 ° C 10 mm 2.0 mm 85 ° C Alloy 7 570 ° C 480 ° C 10 mm 2.0 mm 85 ° C Alloy 8 570 ° C 480 ° C 10 mm 2.0 mm 85 ° C Alloy 9 4.3 mm 2. 5 mm Alloy 10 570 ° C 480 ° C 8 mm 2.0 mm 85 ° C 10 5 Table 2 3036986 13 Tensile tests Tensile tests at room temperature were carried out according to standard NF EN 5 ISO 6892-1 with test pieces no proportional, of widely used geometry for the sheets, and corresponding to the type of specimen 2 of Table B.1 of Annex B of said standard. These specimens have in particular a width of 20 mm and a calibrated length of 120 mm.
[0021] The results of these tensile tests in terms of the 0.2% yield strength, Rpo, 2, and measured on the sheets as manufactured under the conditions described in the preceding paragraph, ie after quenching, pre-tempering, ripening at ambient temperature for a minimum of 72 hours, then strain hardening of 2% in controlled tension to simulate shaping, and hold for 20 min. at 185 ° C to simulate the baking of the paints, are given in Table 3 below. Rpo, 2 [MPa] Alloy 4 217 Alloy 5 264 Alloy 6 282 Alloy 7 288 Alloy 8 291 Invention 1 309 Invention 2 316 Invention 3 307 20 Table 3 It clearly shows that the yield strengths of alloy sheets 1, 2 and 3, according to the invention, are greater than 300 MPa, as claimed, which is not the case for other alloys.
[0022] The results of these tensile tests, again in terms of the 0.2% yield strength, Rpo, 2, but measured on the sheets as manufactured under the conditions described in the previous paragraph, in the T6 state, after quenching, pre-tempering, maturation at room temperature for a minimum of 72 hours, and tempering to reach the T6 state at the peak of hardening, ie 2 hours at 205 ° C., are given in Table 4 below. -after. Rpo, 2 [MPa] Alloy 3 249 Alloy 4 310 Alloy 5 336 Alloy 6 347 Alloy 7 343 Alloy 9 344 Invention 1 355 Invention 2 357 Invention 3 354 10 Table 4 It clearly shows that the yield strengths of alloy sheets 1, 2 and 3, according to the invention, are greater than 350 MPa, as claimed, which is not the case for other alloys.
[0023] Evaluation of ductility in service The ductility in service can be estimated by a "three-point bend test" according to standard NF EN ISO 7438 and procedure VDA 238-100. The folding device is as shown in Figure 1. It is first carried out on a sheet in the T4 state, either after quenching, pre-tempering and maturing at room temperature for 72 hours, a pre-deformation in tension 25 10% controlled in the direction perpendicular to the rolling direction, then held for 20 minutes. at 185 ° C to simulate the firing of the paints, and the "three-point folding" is carried out properly using a punch B of radius r = 0.4 mm, the sheet being supported by two rollers R, the fold axis being perpendicular to the pre-traction direction. The rollers have a diameter of 5 mm and the distance between the axes of the rollers is equal to 30 + 2 mm, where t is the initial thickness of the sheet tested T. At the beginning of the test the punch is brought into contact with the sheet with a pre-force of 30 Newtons. Once the contact is established, the displacement of the punch is indexed to zero. The test then consists in moving the punch so as to effect the "three-point folding" of the sheet. The test stops when a microcracking of the sheet leads to a force drop on the punch of at least 30 Newtons, or when the punch has moved 14.2 mm, which corresponds to the maximum stroke authorized. At the end of the test, the sheet sample is thus folded as illustrated in FIG.
[0024] The ductility in service is then evaluated by measuring the bending angle a, here called aio%, in degrees. The higher the angle θ%, the better the crimping or folding ability of the sheet. The results of these folding tests on the sheets as manufactured according to the conditions described in the "Preamble" paragraph are given in Table 5 below. aio% (°) Alloy 4 63 Alloy 7 52 Invention 1 61 Table 5 It is clearly noted that the angle am% of the sheet according to the invention is greater than 60 °.
[0025] 30 Measurement of LDH (Limit Dome Height) 3036986 16 These measurements of LDH (Limit Dome Height) were carried out in order to characterize the performance in T4 stamping of the various sheets of this example.
[0026] The LDH parameter is widely used for the evaluation of the drawability of sheets of 0.5 to 3.0 mm thickness. He has been the subject of many publications, including that of R. Thompson, "The LDH test to evaluate sheet metal formability - Final Report of the LDH Committee of the North American Deep Drawing Research Group," SAE conference, Detroit, 1993, SAE Paper No. 930815.
[0027] This is a drawing test of a blank blocked at the periphery by a ring. The blanking pressure is controlled to prevent slippage in the rod. The blank, dimensions 120 x 160 mm, is biased in a mode close to the plane strain. The punch used is hemispherical.
[0028] Figure 3 shows the dimensions of the tools used to perform this test. The lubrication between the punch and the plate is ensured by graphited grease (Shell HDM2 grease). The speed of descent of the punch is 50 mm / min. The so-called LDH value is the value of the displacement of the punch at break, the limit depth of the stamping. It actually corresponds to the average of three tests, giving a 95% confidence interval on the 0.2 mm measurement. Table 6 below shows the values of the LDH parameter obtained on test pieces of 120 × 160 mm cut from the above-mentioned sheets with a thickness of 2.5 mm and for which the dimension of 160 mm was positioned parallel to the rolling direction. . LDH (mm) Alloy 8 37.1 Invention 2 36.5 30 Table 6 3036986 17 These results highlight the fact that the sheet according to the invention has an LDH value similar to the value of LDH obtained for an alloy sheet. type AA5182 (alloy 8), reference alloy when it comes to body panels 5 for severe stampings. Evaluation of the corrosion resistance The intergranular corrosion test according to ISO 11846 consists of immersing the test pieces for 24 hours in a solution of sodium chloride (30 g / l) and hydrochloric acid (10 ml / l). at a temperature of 30 ° C (obtained by means of a holding in a drying oven), after stripping with hot soda (5% by weight) and with nitric acid (70% by mass) at room temperature.
[0029] The samples have a dimension of 40 mm (rolling direction) x 30 mm x thickness. The type and depth of corrosion caused is determined by a micrographic sectional examination of the metal. The maximum depth of corrosion is measured.
[0030] The results are summarized in Table 7 below. Maximum depth of attack in! Lm Alloy 9 250 Invention 1 140 Table 7 25 The maximum depth of attack appears significantly lower for the alloy according to the invention, reflecting a better resistance to intergranular corrosion. 30
权利要求:
Claims (14)
[0001]
REVENDICATIONS1. Plate for stamped part of lining, reinforcement or bodywork structure, also known as case in white, aluminum alloy AA6xxx series, composition (% by weight): Si: 0,85 - 1,20 Fe: <0.30 Cu: 0.10 - 0.30 Mg: 0.70 - 0.90 Mn: <0.30 Zn: 1.10 - 1.60 V: 0.05 - 0.30 Ti: 0, 05 - 0.20 other elements <0.05 each and <0.15 in total, remaining aluminum,
[0002]
2. Sheet according to claim 1, characterized in that the Si content is between 0.90 and 1.10%.
[0003]
3. Sheet according to one of claims 1 or 2, characterized in that the Cu content is between 0.10 and 0.20%.
[0004]
4. Sheet according to one of claims 1 to 3, characterized in that the Mg content is between 0.70 and 0.80%.
[0005]
5. Sheet according to one of claims 1 to 4, characterized in that the Zn content is between 1.20 and 1.50%.
[0006]
6. Sheet according to one of claims 1 to 5, characterized in that the V content is between 0.10 and 0.20%.
[0007]
7. Sheet according to one of claims 1 to 6, characterized in that the Ti content is between 0.08 and 0.15%.
[0008]
8. Sheet according to one of claims 1 to 7, characterized in that the Mn content is between 0.10 and 0.20%.
[0009]
9. Sheet according to one of claims 1 to 8, characterized in that the Fe content is between 0.15 and 0.25%. 3036986 19
[0010]
10. A method of manufacturing a sheet according to one of claims 1 to 9, comprising the following steps: 5 - the typical vertical semi-continuous casting of a plate and its possible scalping, - the homogenization of this plate to a temperature of 550 to 570 ° C with a hold between 2 and 12 h, preferably between 4 and 6 h, followed by rapid cooling, - reheating at a temperature between 450 and 550 ° C with a hold between 30 and min and 3 h, preferably substantially 2 h, - the hot rolling of the plate in a strip of thickness between 3 and 10 mm, - the cold rolling to the final thickness, 15 - the dissolution in solution the strip rolled at a temperature above the solvus temperature of the alloy, while avoiding the burn, ie between 550 and 570 ° C for 30 s to 5 min, followed by quenching at a speed of more than 50 ° C / s and preferentially more than 100 ° C / s, - the pre-income, or reversion, by winding at a temperature of at least 60 ° C followed by cooling in the open air of the resulting coil.
[0011]
11. A method of manufacturing a sheet according to one of claims 1 to 9, comprising the following steps: - the typical vertical semi-continuous casting of a plate and scalping 25 possible, - the heating of this plate to a temperature between 550 and 570 ° C with a hold between 2 and 12 h, preferably between 4 and 6 h, - the hot rolling of the plate in a strip of thickness between 3 and 10 mm, - the rolling to cold to the final thickness, - dissolving the rolled strip at a temperature above the solvus temperature of the alloy, while avoiding the burn, ie between 550 and 570 ° C for 30 s 20 to 5 min, followed by quenching at a rate of more than 50 ° C./s and preferably more than 100 ° C./s, the pre-income, or reversion, by winding at a temperature of at least 60.degree. ° C. followed by cooling in the open air of the coil obtained. 5
[0012]
12. Sheet obtained by the method according to one of claims 10 or 11, characterized in that after possible maturation at room temperature between 72 hours and 6 months, a pre-tension deformation controlled 2%, and baking treatment paints, typically 20 min at 185 ° C, it has a yield strength Rpo, 2 of at least 300 MPa.
[0013]
13. Sheet obtained by the process according to one of claims 10 or 11, characterized in that in the metallurgical state T6 according to the European standard EN 515 it has a yield strength Rpo, 2 of at least 350 MPa . 15
[0014]
14. Sheet of a thickness of 2 mm, obtained by the method according to one of claims 10 or 11, characterized in that after optional maturation at room temperature between 72 hours and 6 months, a pre-deformation in traction 10% controlled, and paint curing treatment, typically 20 min at 185 ° C, it has a "three-point bend angle" aio% measured according to the NF EN ISO 7438, and the VDA 238-100 procedure, at least 60 °. 25
类似技术:
公开号 | 公开日 | 专利标题
EP3303646B1|2019-04-24|Metal sheet for a motor vehicle body having high mechanical strength
EP1472380B1|2008-11-05|Al-si-mg alloy sheet metal for motor car body outer panel
EP2750882B1|2018-05-30|Compositealuminium sheet for automotive body shop
EP1633900A1|2006-03-15|Autobody skin piece made of an al-si-mg sheet metal alloy and fixed to a steel structure
WO2015098484A1|2015-07-02|Aluminum alloy plate for molding
EP3317041B1|2019-08-14|Method for the laser welding of monolithic semi-finished products made from aluminium alloy, without filler wire, and corresponding structural component and tailored blank
EP3362282B1|2020-01-01|Structural component of a motor vehicle shell offering an excellent compromise between mechanical strength and crash resistance
CA3057728A1|2018-10-11|Improved method for producing a motor vehicle body structure component
CA3006346A1|2017-06-08|Highly rigid thin sheet metal for car body
EP3019637B1|2017-05-03|Sheet made of aluminum alloy for the structure of a motor vehicle body
KR20170038857A|2017-04-07|Aluminum alloy sheet
EP3555331B1|2021-07-14|Aluminium alloy for laser welding without filler wire
WO2020016506A1|2020-01-23|Process for manufacturing thin sheets made of 7xxx aluminum alloy suitable for shaping and assembly
同族专利:
公开号 | 公开日
EP3303646B1|2019-04-24|
CN107709590A|2018-02-16|
CN107709590B|2020-10-13|
AR104913A1|2017-08-23|
US20180179621A1|2018-06-28|
US10829844B2|2020-11-10|
KR20180016375A|2018-02-14|
RU2017145569A|2019-07-09|
WO2016193640A1|2016-12-08|
EP3303646A1|2018-04-11|
BR112017023524A2|2018-07-24|
TR201907640T4|2019-06-21|
FR3036986B1|2017-05-26|
JP2018521229A|2018-08-02|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
JPH05112840A|1991-10-18|1993-05-07|Nkk Corp|Baking hardenability al-mg-si alloy sheet excellent in press formability and its manufacture|
US5888320A|1995-05-11|1999-03-30|Kaiser Aluminum & Chemical Corporation|Aluminum alloy having improved damage tolerant characteristics|
US6231809B1|1998-02-20|2001-05-15|Kabushiki Kaisha Kobe Seiko Sho |Al-Mg-Si aluminum alloy sheet for forming having good surface properties with controlled texture|
DE60108382T3|2000-06-01|2010-03-18|Alcoa Inc.|CORROSION RESISTANT ALLOYS OF THE 6000 SERIES USEFUL FOR AVIATION|
JP4115936B2|2001-07-09|2008-07-09|コラス・アルミニウム・バルツプロドウクテ・ゲーエムベーハー|Weldable high strength Al-Mg-Si alloy|
JP4101749B2|2001-07-23|2008-06-18|コラス・アルミニウム・バルツプロドウクテ・ゲーエムベーハー|Weldable high strength Al-Mg-Si alloy|
JP2003268475A|2002-03-12|2003-09-25|Sky Alum Co Ltd|Aluminum alloy sheet for forming, and manufacturing method therefor|
FR2856368B1|2003-06-18|2005-07-22|Pechiney Rhenalu|BODY PIECE OF AUTOMOBILE BODY IN ALLOY SHEET AI-SI-MG FIXED ON STRUCTURE STEEL|
DE102005045340B4|2004-10-05|2010-08-26|Aleris Aluminum Koblenz Gmbh|Process for heat treating an aluminum alloy element|
JP2006322064A|2005-04-19|2006-11-30|Furukawa Electric Co Ltd:The|High moldability aluminum material|
JP4939093B2|2006-03-28|2012-05-23|株式会社神戸製鋼所|Method for producing 6000 series aluminum alloy plate for automobile panel having excellent hem bendability and bake hardness|
CN104080935A|2011-11-02|2014-10-01|株式会社Uacj|Aluminum alloy clad material for molding|EP3400316B1|2016-01-08|2020-09-16|Arconic Technologies LLC|New 6xxx aluminum alloys, and methods of making the same|
US10835942B2|2016-08-26|2020-11-17|Shape Corp.|Warm forming process and apparatus for transverse bending of an extruded aluminum beam to warm form a vehicle structural component|
MX2019004494A|2016-10-24|2019-12-18|Shape Corp|Multi-stage aluminum alloy forming and thermal processing method for the production of vehicle components.|
US10030295B1|2017-06-29|2018-07-24|Arconic Inc.|6xxx aluminum alloy sheet products and methods for making the same|
CN108754363A|2018-06-22|2018-11-06|中南大学|Regulate and control the method for aluminium alloy element stress relaxation behavior|
CN112941432A|2019-11-26|2021-06-11|晟通科技集团有限公司|6-series aluminum profile and heat treatment process thereof|
法律状态:
2016-06-28| PLFP| Fee payment|Year of fee payment: 2 |
2016-12-09| PLSC| Search report ready|Effective date: 20161209 |
2017-06-27| PLFP| Fee payment|Year of fee payment: 3 |
2018-06-26| PLFP| Fee payment|Year of fee payment: 4 |
2020-06-25| PLFP| Fee payment|Year of fee payment: 6 |
2021-06-25| PLFP| Fee payment|Year of fee payment: 7 |
优先权:
申请号 | 申请日 | 专利标题
FR1555129A|FR3036986B1|2015-06-05|2015-06-05|BODY FOR CAR BODY WITH HIGH MECHANICAL STRENGTH|FR1555129A| FR3036986B1|2015-06-05|2015-06-05|BODY FOR CAR BODY WITH HIGH MECHANICAL STRENGTH|
JP2018515356A| JP2018521229A|2015-06-05|2016-06-03|Thin plate for automobile body with high mechanical strength|
BR112017023524A| BR112017023524A2|2015-06-05|2016-06-03|sheet metal for automotive bodywork with high mechanical strength|
US15/578,735| US10829844B2|2015-06-05|2016-06-03|Metal sheet for a motor vehicle body having high mechanical strength|
PCT/FR2016/051333| WO2016193640A1|2015-06-05|2016-06-03|Metal sheet for a motor vehicle body having high mechanical strength|
CN201680032817.4A| CN107709590B|2015-06-05|2016-06-03|Sheet metal for motor vehicle bodies having high mechanical strength|
EP16735908.2A| EP3303646B1|2015-06-05|2016-06-03|Metal sheet for a motor vehicle body having high mechanical strength|
TR2019/07640T| TR201907640T4|2015-06-05|2016-06-03|Sheet for high mechanical strength car body.|
ARP160101672A| AR104913A1|2015-06-05|2016-06-03|PLATE FOR CAR BODY WITH HIGH MECHANICAL RESISTANCE AND MANUFACTURING PROCESS|
RU2017145569A| RU2017145569A|2015-06-05|2016-06-03|SHUTTER FOR BODY CAR WITH HIGH MECHANICAL STRENGTH|
KR1020177034946A| KR20180016375A|2015-06-05|2016-06-03|A metal sheet for an automobile body having high mechanical strength|
[返回顶部]