专利摘要:
A dry particulate composition for forming a geopolymer, comprising an alkali metal hydroxide, an alkali metal silicate and an aluminosilicate, wherein at least 45% by weight of the aluminosilicate is in an amorphous state based on the total weight of aluminosilicate in the composition and the aluminosilicate has a surface area product in m 2 / g by the amorphous phase content in the range of 1 to 15.
公开号:FR3033165A1
申请号:FR1600333
申请日:2016-02-29
公开日:2016-09-02
发明作者:Alexandre Autef
申请人:Imerys Ceramics France;
IPC主号:
专利说明:

[0001] PARTICULAR COMPOSITIONS FOR THE FORMATION OF GEOPOLYMERS, THEIR USE AND METHOD FOR FORMING GEOPOLYMERS AND GEOPOLYMERS OBTAINED THEREFROM FIELD OF THE INVENTION [1] The present invention relates to geopolymers in a general and precise manner. to dry particulate compositions to form geopolymers. The use of these dry particulate compositions and the methods for making geopolymers also form part of the present invention, as well as geopolymer precursors and the finished geopolymers derived therefrom. BACKGROUND OF THE INVENTION [2] A new class of materials has emerged as geopolymers in cement and concrete products. Geopolymers are not only considered to be a potential substitute for conventional cement, but they also provide the opportunity to turn various industrial wastes into valuable by-products. As geopolymers can have good mechanical strength and withstand aggressive operations, they are currently very interested in their potential use to simultaneously improve both environmental and technical performance compared to conventional technologies. Geopolymers are normally formed by polymerizing aluminosilicate oxides in the presence of a very basic activating agent. According to the state of the art, the polymerization is initiated by a liquid alkali silicate. This is favored, in general, by the reaction mechanisms, as described in the scientific literature. Next Fernandez-Jiménez A. et al. (Cernent and Concrete Research, 35 (6), pages 1204 to 1209, 2005) A dissolution of a solid aluminosilicate by alkaline hydrolysis is the first stage of reaction and leads to the formation of aluminates and silicates. After a formation equilibrium is obtained, a saturated solution is formed which leads to an oligomer network, which has undergone polycondensation to form a three-dimensional network of aluminosilicates. This process requires a very large amount of water, which is then removed in part from the product. [03] Recently, research has focused on obtaining precursors to form geopolymers, which can be easily stored, handled and transported to obtain the finished product on site where it is needed. Ideally, the finished product can be obtained by simply adding water to a precursor and thereby forming a geopolymer. [04] US 2011/0132230 A1 (Han et al.) Discloses dry mixtures as geopolymeric precursors comprising a water-soluble metal silicate powder and an aluminosilicate powder. The geopolymer precursors may further include additional ingredients such as, for example, but not necessarily, a particulate solid alkaline base. These dry blends require adding a large amount of water to give a geopolymer. In addition, the aluminosilicate present requires a large amorphous phase content, such as greater than or equal to 90% by weight. The present invention is directed to a dry blend with little need for water to form geopolymers having the desired mechanical properties. [6] The present invention further provides a method of preparing a geopolymer on site just by adding water. DESCRIPTION OF THE INVENTION [7] The present invention relates to the dry particulate composition for forming a geopolymer comprising: (i) an alkali metal hydroxide, (ii) an alkali metal silicate and (iii) an aluminosilicate, wherein at least 45% by weight of the aluminosilicate is in an amorphous state based on the total weight of aluminosilicate in the composition and the aluminosilicate has a product of the specific surface area in m2 / g by the amorphous phase content in the range of 1 to 15: Preferably: at least 50% by weight of the aluminosilicate is in an amorphous state; the dry particulate composition comprises from 1% by weight to 25% by weight of alkali metal hydroxide, from 15% by weight to 50% by weight of alkali metal silicate and from 30% by weight to 80% by weight aluminosilicate expressed as a proportion of the total weight of the dry particulate composition; the alkali metal hydroxide is selected from the group consisting of NaOH, KOH, LiOH, RbOH, CsOH and mixtures thereof; The alkali metal of the alkali metal silicate is selected from the group consisting of Na, K, Li, Rb, Cs and mixtures thereof; the aluminosilicate is selected from the group consisting of metakaolin, fly ash, halloysite, metahalloysite, slag, powdered rock, fine sand, activated clay, kaolin, mica, feldspar end and their mixtures; at least 50% by weight of the aluminosilicate is in an amorphous phase with respect to the total weight of aluminosilicate in the composition and the aluminosilicate has a product of the specific surface area in m 2 / g by the amorphous phase content in the range from 5 to 15; At least 70% by weight of the aluminosilicate is in an amorphous phase relative to the total weight of aluminosilicate in the composition and the aluminosilicate has a product of the specific surface area in m 2 / g by the amorphous phase content in 20 the range of 10 to 15; the aluminosilicate has a product of the specific surface area in m 2 / g by the amorphous phase content in the range of 7 to 15 or 8 to 15 or 10 to 15.
[0002] The invention also relates to a process for preparing a geopolymer comprising the step of mixing a dry particulate composition according to the invention with water. Preferably: the amount of water is less than or equal to 50% by weight or in the range of 10% by weight to 50% by weight relative to the total weight of the particulate composition and water; The dry particulate composition further comprises the step of adding aggregates after the addition of water and before the geopolymerization of the mixture.
[0003] The invention also relates to a geopolymer obtained from a dry particulate composition according to the invention or by a process according to the invention. The invention also relates to the use of the composition 10 according to the invention or the process according to the invention in the production of products or objects selected from mortars, concretes, cements, coatings, management objects. waste for immobilization of toxic or nuclear waste, fiber-reinforced / high-tech geopolymer composites, geopolymeric foams, for example for insulation, incombustible coatings of foundry equipment, bricks, resins, binders, roads or sidewalks and the use of an aluminosilicate to prepare. The invention finally relates to a dry particulate composition for forming a geopolymer, at least 45% by weight of the aluminosilicate being in an amorphous state based on the total weight of aluminosilicate in the composition and the aluminosilicate has a product of 25% by weight. the specific surface area in m 2 / g by the amorphous phase content in the range of 1 to 15. The first embodiment of the present invention is directed to a dry particulate composition to form a geopolymer. This dry particulate composition may also be referred to as dry mix or premix to form a geopolymer. [08] In particular, the present invention is incorporated into a dry particulate composition to form a geopolymer comprising an alkali metal hydroxide, an alkali metal silicate and an aluminosilicate, at least 45% by weight of the aluminosilicate being in an amorphous state with respect to the total weight of the aluminosilicate in the composition, such as, for example, when at least 50% by weight of aluminosilicate is in an amorphous state. These compositions have been found to have improved properties in terms of ease of handling and preparation of the finished geopolymer on site. [09] In a separate embodiment, the present invention is a dry particulate composition to form a geopolymer comprising an alkali metal hydroxide, an alkali metal silicate and an aluminosilicate, the aluminosilicate having a surface product specific (in m2 / g) by the amorphous phase content in the range of 1 to 15 such as, for example, 5 to 15. It has been found that these compositions have improved properties in terms of ease of handling. [10] In one embodiment of the present invention, the dry particulate composition may comprise from 1% by weight to 25% by weight of alkali metal hydroxide, from 15% by weight to 50% of alkali metal silicate and from 30% by weight to 80% by weight of aluminosilicates, each expressed as a proportion of the total weight of the dry particulate composition. It has been found that, depending on the origin and the quality of the raw materials used, the best results are obtained by using the constituents of the composition according to the present invention in these amounts. [11] In one embodiment of the present invention, the alkali metal hydroxide in the dry particulate composition may be selected from the group consisting of NaOH, KOH, LiOH, RbOH, CsOH and mixtures thereof. It has been found that these alkali metal hydroxides give the best results in practice. [12] In one embodiment of the present invention, the aluminosilicate of the dry particulate composition can be selected from the group consisting of metakaolin, fly ash, halloysite, metahalloysite, slag, powdered rock. , fine sand, activated clay, kaolin, mica, fine feldspar and mixtures thereof. These aluminosilicates have been found to give the best results in practice. As used herein, aluminosilicates are minerals composed of aluminum, silicon and oxygen. Depending on their origin, the Al, Si and O content of the aluminosilicate may vary as well as the content of inert constituents (eg quartz, cristobalite, mullite, muscovite, mica, anatase, rutile, kaolinite, albite, orthoclase). [13] In one embodiment of the present invention, the dry particulate composition may further comprise a filler selected from the group consisting of mica, refractory clay, quartz, quartz sands, silica, and the like. fumed silica, talc, andalusite, wollastonite, glass pellets, fibers or mixtures thereof. [14] Also part of the present invention is a process for preparing a geopolymer comprising the step of mixing the dry particulate composition of the present invention with water. It has been found that this method makes it easier to give finished geopolymers on site by combining the advantages of the compositions according to the present invention with a reduced need for water to obtain the finished product. [15] According to one embodiment of the present invention, the amount of water is less than 50% by weight, for example in the range of 10% by weight to 50% by weight such as, for example, in the range of 15% by weight 5 to 50% by weight relative to the total weight of the particulate composition and water. It has been found that the best results for the final geopolymer product can thus be obtained. [16] According to one embodiment of the present invention, this method of preparing a geopolymer at a temperature between 0 ° C and 100 ° C and using any type of water such as distilled water or tap water. It has been found that the process according to the present invention can be used in a wide temperature range and without particular requirements on the origin of the water on site. According to one embodiment of the present invention, the method of preparing a geopolymer may comprise the further step of adding aggregates or other additives after addition of water and prior to geopolymerization of the mixture. . [18] Also part of the present invention is a geopolymer composition, obtained by using a dry particulate composition to form a geopolymer according to the present invention or a method of preparing a geopolymer according to the present invention or both, as well as the use of geopolymers in the production of objects, objects incorporating geopolymers. It has been found that the geopolymers obtained according to the present invention provide advantages in that. the handling of the precursor materials and the method of obtaining the actual product on site, while 3033165 having all the advantageous properties of the geopolymers of the state of the art. BRIEF DESCRIPTION OF THE DRAWINGS [19] The invention will be further illustrated with reference to the following figure: Figure 1 is a graph showing the relationship between the amorphous phase content and the product of the specific surface area (in m2 / g ) by the amorphous phase content of the samples used in Examples 1 to 9 and Comparative Examples 1 to 6. [20] It goes without saying that what is described hereinafter and with reference to FIGS. This invention relates to exemplary embodiments of the present invention and should not be construed as limiting the scope. DETAILED DESCRIPTION OF THE INVENTION [21] The present invention provides, in one embodiment, precursor compositions useful in the production of geopolymeric materials. The precursor compositions according to the present invention are dry particulate compositions which can be used to form a geopolymer by the addition of water. The main advantage of the composition according to the present invention lies in the elimination of the use of strong and corrosive basic alkaline solutions at the moment when the geopolymer 30 itself is formed. In addition, the time to obtain the finished geopolymer on site is reduced due to the single-stage process of mixing the precursor with water, the reaction not requiring the decomposition stage of oligopolymers present in the process. alkali metal silicate solution. According to the present invention, a geopolymer can be obtained by combining a mixture of particulate geopolymer precursors and water. The present invention relies on the principle of different solubility rates of the various constituents of the dry particulate precursor. Alkaline sources (alkali metal hydroxide and alkali metal silicate) do not have to have a faster dissolution rate in water in order to come into solution more rapidly and provide a reaction mixture for dissolving the aluminosilicate. [23] According to the present invention, the geopolymer precursor compositions are suitable for a dissolution-geopolymerization process comprising the steps of (i) rapidly dissolving the alkaline source to provide a very basic reaction mixture (pH> 12) and (ii) ) Limited reaction rate of the aluminosilicate to permit dissolution of the aluminosilicate only after dissolution of the alkaline sources. Successive dissolutions of the various precursors result in a reaction mixture in which a geopolymerization reaction occurs at temperatures between 0 ° C and 100 ° C. [24] The reactivity rate of the aluminosilicate may depend among other factors on the relative amount of amorphous phase in the aluminosilicate. The amorphous phase content is dependent on the amount of species which can be dissolved in a basic medium and which can then participate in the geopolymerization reaction. The amount of amorphous phase is determined by X-ray diffraction (improved Rietveld method). According to one embodiment of the invention, the amorphous phase content may be at least 45% by weight relative to the total weight of aluminosilicate in the composition. The amorphous phase content of the aluminosilicate may be, for example, at least 50% by weight, at least 55% by weight, at least 60% by weight or at least 70% by weight or at least 80% by weight or even at least 90% by weight of the total weight of aluminosilicate in the composition. [25] The reactivity rate of the aluminosilicate may also depend on the surface area of the aluminosilicate. A larger surface area of the aluminosilicate gives a higher reaction rate. It has been found, surprisingly, that the product of the surface area by the amorphous phase content of the aluminosilicate has a good correlation with the ability of the aluminosilicate to provide additional advantages in accordance with the present invention. According to one embodiment of the invention, it is therefore required that the product of the surface area (in m 2 / g) by the amorphous phase content be in the range of 1 to 15 such as, for example, at 15 or from 7 to 15 or from 8 to 15 or from 10 to 15. If the product of the specific surface (in m 2 / g) by the amorphous phase content and too small, a geopolymerization does not take place, because the amount of amorphous phase is not sufficient. If the product is greater than 15, the reaction is not complete, and the products obtained are non-geopolymeric species having a very small cohesion and insufficient mechanical properties. [26] Aluminosilicates for use in the present invention can be obtained by grinding the raw materials. In the case of kaolin, the particulate material can then be calcined using, for example, an oven or kiln calcination, or using fly ash calcination. The particulates are then finally sized according to size using a screen or wire cloth or air separator to, for example, break up or filter out any aggregate above a certain diameter, which was formed. The aluminosilicate particles may still be in the form of aggregates or particles, although the aggregates or particles have a maximum maximum cutting diameter (duo). [27] According to one embodiment of the present invention, the aluminosilicate aggregates have a D100 dimension of less than 300 μm or less than 200 μm or less than 150 μm, such as for example less than 120 μm. or less than 100 pm or less than 90 pm or less than 80 pm. According to another embodiment, the aluminosilicate aggregates are such that at least 95% have a D100 dimension of less than 300 μm or less than 200 μm, for example at least 97%, at least 98% or at least 98%. 99%. According to another embodiment, the aluminosilicate aggregates are such that at least 90% have a D100 dimension of less than 200 μm or less than 150 μm, for example at least 95%, at least 97% or at least 99%. According to another embodiment, the aluminosilicate aggregates are such that at least 80% have a D100 dimension of less than 100 μm, for example at least 85%, at least 90% or at least 95%. As used herein, a particle size of less than 300 micrometers requires that after calcination the aluminosilicate aggregates have passed through, for example, a sieve, wire mesh or air separator. a diameter of 300 μm effectively giving an upper cut of particle diameter of 300 μm. The same applies to all other particle size values. [28] According to the present invention, a geopolymer material can be formed by adding water to the dry particulate composition. The amount of water introduced into the dry particulate composition should be such that the water content of the resulting mixture of particulate material and water is less than 50% by weight, for example from 10% by weight to 50% in weight. The amount of water may range, for example, from 15% by weight to 40% by weight or the amount of water may range, for example, from 20% by weight to 35% by weight, such as by 25% by weight or about 28% by weight or about 30% by weight or about 32% by weight. These amounts of water provide ideal conditions for dissolving all species and for the geopolymerization reaction to be complete. If there is not enough water, all the species (Si and Al) are not dissolved because the reaction medium becomes saturated and the geopolymerization reaction remains incomplete. If there is too much water, the pH of the reaction mixture will drop and the dissolution of all species will not be reached. In addition, the small Si and Al species concentration limits the bond formation between the atoms and thus prevents the formation of a geopolymer network. The geopolymerization reaction remains incomplete again. [29] According to the present invention, the aluminosilicate may be selected from the group consisting of metakaolin, fly ash, haloysite, metahalloysite, slag, powdered rock, fine sand, activated clay and their mixtures. All these aluminosilicates have advantageous properties. It is particularly advantageous for the present invention to use an aluminosilicate requiring little water. In one embodiment, the aluminosilicate to be used in the invention is a metakaolin. [30] According to the present invention, the alkali metal hydroxide may be one of NaOH, KOH, LiOH, RbOH, or CsOH or a mixture thereof. The preferred alkali metal hydroxides are NaOH, KOH and LiOH. [31] According to the present invention, the alkali metal silicate for use in the dry particulate composition may be selected from the group consisting of Na, K, Li, Rb, Cs and mixtures thereof. In particular, the alkali metal silicate may be sodium silicate, sodium metasilicate (waterglass) and / or potassium silicate. [32] According to one embodiment of the present invention, the dry particulate composition to form a geopolymer comprises: (i) NaOH as the alkali metal hydroxide, (ii) sodium silicate as the alkali metal silicate and (iii) ) metakaolin as aluminosilicate, at least 45% by weight of the metakaolin being in the amorphous state relative to the total weight of the metakaolin in the composition and the metakaolin to a product of the specific surface area in m2 / g by the phase content In another embodiment of the present invention, the dry particulate composition for forming a geopolymer comprises (i) NaOH as the alkali metal hydroxide (ii), sodium silicate as the alkali metal silicate (iii), metakaolin 30 as aluminosilicate, at least 45% by weight of the metakaolin being in the amorphous state relative to the total weight of the metakaolin in the composition and the metakaolin to a pro the surface area in m2 / g is the amorphous phase content in the range of 10 to 15. [34] According to yet another embodiment of the present invention, the particulate composition dries to form a geopolymer of the The present invention comprises (i) an alkali metal hydroxide, (ii) an alkali metal silicate and (iii) an aluminosilicate-containing compound at least 45% by weight of the aluminosilicate being in the amorphous state with respect to the weight total aluminosilicate in the composition and the aluminosilicate has a product of the specific surface area in m2 / g by the amorphous phase content in the range of 1 to 15, excluding an aluminosilicate having a phase content 68.9% amorphous relative to the total weight of aluminosilicate in the composition and a product of the specific surface area in m2 / g by the amorphous phase content of 9.78. [35] According to the present invention, the composition particulate matter may include a or multiple fillers in the group consisting of mica, refractory clay, quartz, quartz sands, fumed silica, talc, andalusite, wollastonite, glass pellets, fibers or mixtures thereof. [36] According to the present invention, the dry particulate composition can comprise from 1 wt.% To 25 wt.% Alkali metal hydroxide, 15 wt.% To 50 wt.% Alkali metal silicate, and 30 wt. % by weight to 80% by weight of aluminosilicate expressed as a proportion of the total weight of the dry particulate composition. The dry particulate composition may comprise, for example, from 2% to 15% by weight of alkali metal hydroxide or from 5% by weight to 10% by weight of alkali metal hydroxide, such as, for example, about 6% by weight of alkali metal hydroxide or about 7% by weight of alkali metal hydroxide or about 8% by weight of alkali metal hydroxide, or about 9% by weight of alkali metal hydroxide. The dry particulate composition may also comprise, for example, from 20% by weight to 40% by weight of alkali metal silicate such as from 25% by weight to 35% by weight of alkali metal silicate, for example about 28% by weight of alkali metal silicate or about 30% by weight of alkali metal silicate or about 32% by weight of alkali metal silicate. The dry particulate composition may also comprise, for example, from 40 to 75% by weight of aluminosilicate or from 50 to 70% by weight of aluminosilicate or from 55 to 65% by weight of aluminosilicate, such as for example about 58% by weight of aluminosilicate or about 60% by weight of aluminosilicate or about 62 by weight of aluminosilicate. [37] According to the present invention, a method for forming a geopolymer using one of the dry particulate compositions described above also forms a part of the invention. The method comprises adding water to the dry particulate composition, the amount of water being such that the water content of the resulting mixture of particulate matter and water can be less than 50% by weight, such as from 10% by weight to 50% by weight or from 15% by weight to 50% by weight. After addition of water, the alkali metal hydroxide and the alkali metal silicate are rapidly passed into solution, which is an exothermic process and a rise in temperature is detected. After homogenization of the mixture, it is allowed to react and, after no more than 24 hours, such as for example after 12 hours, a finished geopolymer product is formed. Aggregates or other materials may be added to the homogenized mixture prior to geopolymerization if necessary. [38] The dry particulate compositions of the present invention can be used in the formation of two geopolymers for use in the production of various products and articles, such as, for example, mortars, concretes, cements, waste management for immobilization of toxic or nuclear wastes, high-tech / fiber-reinforced composites, geopolymeric foams, eg for the insulation of non-combustible coatings, foundry equipment, bricks, resins binders, roads, sidewalks or the like. These products and objects also form a part of the present invention. [39] Also part of the present invention is a geopolymer comprising 50% by weight or more of the dry particulate composition according to the present invention and up to 50% by weight of water. The geopolymer may comprise, for example, 60% by weight or more of the dry particulate composition of the present invention and up to 40% by weight water or the geopolymer may comprise 70% by weight or more of the particulate composition according to the present invention and up to 30% by weight of water, or the geopolymer may comprise 80% by weight or more of the dry particulate composition according to the present invention and up to 20% by weight of water, or the geopolymer may comprise 90% by weight or more of the dry particulate composition of the present invention and up to 10% by weight of water. [40] Note that the present invention may include any combination of features and / or limitations mentioned herein except where combinations of such features are mutually exclusive. The foregoing description is directed to particular embodiments of the present invention for purposes of illustration. But it is clear to those skilled in the art that many modifications and variations can be made to the embodiments described herein. It is meant that all such modifications and variations are within the scope of the present invention. EXAMPLES Examples 1 to 9 [41] A number of commercially available aluminosilicates (listed here as Comparative Examples 1 to 6 and Examples 1-9) for use in a dry particulate composition according to the present invention were tested in accordance with the present invention. forming geopolymers using these aluminosilicates under otherwise constant conditions. The kaolin used in Examples 1, 3, 6, 8 and Comparative Example 6 were calcined at 750 ° C for 3 hours. After calcination, the products were sieved at 80 μm. Metakaolins are used in Comparative Examples 1 to 5 and Examples 2, 4, 5, 7 and 9. The properties of these aluminosilicates are listed in Table I and their origins are listed in Table II: TABLE I: Property of aluminosilicates Phase amorphous (% by weight) Specific surface area Product (m2 / g) ap x ssa Comp. Ex. 1 43.3 3.7 1.60 Comp. Ex. 2 39.5 7.0 2.76 Example 1 94.5 8.7 7.24 Example 2 56.2 15.2 8.54 3033165 19 Example 3 68.9 14.2 9.78 Example 4 75 13.6 10.24 Example 5 91.8 13.9 12.76 Example 6 95.4 14.7 14.02 Example 7 95.0 14.9 14.15 Example 8 90.7 16.0 14 , Example 9 83.6 17.7 14.80 Comp. Ex. 3 97.0 15.6 15.13 Camp. Ex. 4 98.0 16.6 16.27 Camp. Ex. 5 74.9 22.00 16.48 Camp. Ex. 6 98.0 19.2 18.82 "The product ap x ssa" is the product of the specific surface area in m2 / g by the amorphous phase content. TABLE II: Aluminosilicate Trade Name Supplier Camp. Ex. 1 Metakaolin METASIAL B SOCIETY KAOLINIERE ARMORICAINE (SOKA) Camp. Ex. 2 Metakaolin Argicem Argeco Example 1 Kaolin Remblend Imerys Example 2 Metakaolin Metaver R NEWCHEM AG Example 3 Kaolin Pioneer Imerys Example 4 Metakaolin MK40 Imerys Example 5 Metakaolin Metakaolin S Meta 4 Sedlecky-kaolin Example 6 Kaolin (Non-commercial) Imerys Example 7 metakaolin Metakaolin N Meta 4 Sedlcky-kaolin Example 8 Kaolin Hywite HK2 Imerys Example 9 metakaolin Metakaolin I Meta 4 Sedlecky-kaolin Camp. Ex. 3 metakaolin Polestar450 Imerys Camp. Ex.4 metakaolin Metastar501 Imerys Camp. Ex. 5 Metakaolin Argical-M 1200S Imerys Camp. Ex.
[0004] Kaolin SBF Imerys [42] The amount of amorphous phase in the aluminosilicate can be determined, for example, by quantitative X-ray diffraction, as obtained by obtaining an X-ray diffractogram on non-aluminosilicate powder. oriented at less than 40 μm with 20% of zincite as internal gauge and by diffractogram modeling by Topas software (Bruker). [43] As used herein the "specific surface" refers to the BET specific surface area.
[0005] As used herein, "BET surface area" refers to the technique for calculating the surface area of physically absorbing molecules according to the Brunauer, Emmett and Teller ("BET") theory. The BET specific surface area can be measured by a Gemini III 2375 specific surface analyzer, using nitrogen as an absorbent gas, from Micromeritics Instrument Corporation (Norcross, Ga., USA). [44] The aluminosilicates of Comparative Examples 1 and 2 have an amorphous phase content outside the scope of the present invention. The aluminosilicates of Comparative Examples 3 to 6 have a surface area product in m 2 / g by the amorphous phase content outside the scope of the present invention. All aluminosilicates according to Examples 1 to 9 have an amorphous phase content and a product of the specific surface area in m 2 / g by the amorphous phase content within the scope of the present invention. [45] All samples were used in a method for preparing a geopolymer in a manner similar to that described in Example 10 below. It has been found that for Examples 1 to 9 a geopolymer is formed according to the process of the present invention consisting essentially of the addition of water to a particular dry composition according to the present invention having aluminosilicate. as selected according to Table I. In Comparative Examples 1 and 2, no consolidation reaction was observed. Consolidation of the mixture was observed in Comparative Examples 3 to 6, but the product was not a geopolymer and the resulting material had reduced cohesion and mechanical properties which were unsatisfactory (eg bending less than 1 MPa). In contrast, the geopolymer prepared using an aluminosilicate according to any of Examples 1 to 9 has satisfactory mechanical properties (eg, flexural strength greater than 1 MPa).
[0006] Example 10 [46] A dry particulate composition was formed according to the present invention using a metakaolin (corresponding to Example 8 above), sodium silicate powder ("Britesil C205", supplied by PQ 15 Corporation) and fine pellets of sodium hydroxide (supplied by Sigma Aldrich). The metakaolin used was provided by IMERYS and has a composition of 5102 (50.2%), Al2O3 (39.6%), K20 (0.62%), Na2O (0.01%) and other constituents (8.22%). , 7%), with a loss on ignition of 0.9%. The particulate composition was manually mixed and had a metakaolin composition (61.6% by weight), sodium hydroxide (7.6% by weight) and sodium silicate (30.75%). [47] Water was added and the mixture was homogenized by mechanical stirring. The amount of water added was such that the final composition would theoretically have the following proportions: metakaolin (42.57% by weight), sodium hydroxide (5.28% by weight), sodium silicate (21.25%), and water (30.90% by weight). After homogenization, the mixture warms from room temperature to about 55 ° C, due to the exothermic dissolution of sodium hydroxide and sodium silicate in water. The reaction mixture is then placed in a sealed tube for 22 hours. After removing the reaction mixture from the tube, the product cured. The product obtained was crushed and both the ground product and the starting metakaolin were analyzed by X-ray diffraction. [48] The starting metakaolin diffractogram shows a broad, unsymmetrical peak characteristic of an amorphous phase between 20 and 35 ° (20), with a maximum at about 25 °. In the product composition, this peak shifted to 25-40 ° with a maximum at about 35 °.
[0007] This shows that a geopolymer species had formed in the process of this invention. 15
权利要求:
Claims (15)
[0001]
REVENDICATIONS1. A dry particulate composition for forming a geopolymer, comprising: (i) an alkali metal hydroxide (ii) an alkali metal silicate and (iii) an aluminosilicate, wherein at least 45% by weight of the aluminosilicate is in a amorphous state relative to the total weight of aluminosilicate in the composition and the aluminosilicate has a product of the specific surface area in m2 / g by the amorphous phase content in the range of 1 to 15.
[0002]
The dry particulate composition of claim 1, wherein at least 50% by weight of the aluminosilicate is in an amorphous state. 20
[0003]
3. A dry particulate composition according to any one of the preceding claims, comprising from 1% by weight to 25% by weight of alkali metal hydroxide, from 15% by weight to 50% by weight of alkali metal silicate and from 30% by weight of alkali metal hydroxide. % by weight to 80% by weight of aluminosilicate expressed as a proportion of the total weight of the dry particulate composition.
[0004]
4. Dry particulate composition according to any one of the preceding claims, wherein the alkali metal hydroxide is selected from the group consisting of NaOH, KOH, LiOH, RbOH, CsOH and mixtures thereof. 3033165 24
[0005]
A dry particulate composition according to any one of the preceding claims wherein the alkali metal of the alkali metal silicate is selected from the group consisting of Na, K, Li, Rb, Cs and mixtures thereof.
[0006]
The dry particulate composition according to any one of the preceding claims, wherein the aluminosilicate is selected from the group consisting of metakaolin, fly ash, halloysite, metahalloysite, slag, powdered rock, fine sand , activated clay, kaolin, mica, fine feldspar and mixtures thereof.
[0007]
A dry particulate composition according to any one of the preceding claims, wherein at least 50% by weight of the aluminosilicate is in an amorphous phase based on the total weight of aluminosilicate in the composition and the aluminosilicate has a product of the specific surface area in m2 / g by the amorphous phase content in the range of 5 to 15.
[0008]
A dry particulate composition according to any one of the preceding claims, wherein at least 70% by weight of the aluminosilicate is in an amorphous phase based on the total weight of aluminosilicate in the composition and the aluminosilicate has a product. the specific surface area in m2 / g by the amorphous phase content in the range of 10 to 15.
[0009]
The dry particulate composition according to any one of claims 1 to 7, wherein the aluminosilicate has a surface area product in m 2 / g by the amorphous phase content in the range of 7 to 15 or 8 to 15 or 10 to 15. 5
[0010]
A process for preparing a geopolymer comprising the step of mixing a dry particulate composition as claimed in any one of the preceding claims with water. 10
[0011]
11. A process according to claim 10 wherein the amount of water is less than or equal to 50% by weight or in the range of 10% by weight to 50% by weight based on the total weight of the particulate composition and 'water. 15
[0012]
The process of claim 10 or 11, further comprising the step of adding aggregates after the addition of water and before the geopolymerization of the mixture. 20
[0013]
13. A geopolymer obtained from a dry particulate composition as claimed in any one of claims 1 to 9 and / or a process as claimed in any one of claims 10 to 12.
[0014]
14. Use of the composition according to any one of claims 1 to 9 or the process according to any one of claims 10 to 12, in the production of products or objects selected from mortars, concretes, cements, coatings, waste management objects for immobilization of toxic or nuclear waste, fiber-reinforced / high-tech geopolymer composites, geopolymeric foams, for example for insulation, incombustible coatings, foundry equipment, bricks, resins, binders, roads or sidewalks. 5
[0015]
15. Use of an aluminosilicate to prepare a dry particulate composition to form a geopolymer, at least 45% by weight of the aluminosilicate being in an amorphous state based on the total weight of aluminosilicate in the composition and aluminosilicate has a product of the specific surface area in m2 / g by the amorphous phase content in the range of 1 to 15.
类似技术:
公开号 | 公开日 | 专利标题
FR3033165A1|2016-09-02|
Mijarsh et al.2014|Synthesis of geopolymer from large amounts of treated palm oil fuel ash: application of the Taguchi method in investigating the main parameters affecting compressive strength
EP2467349B1|2019-08-07|Geopolymer cement and use thereof
Al Bakri et al.2012|The processing, characterization, and properties of fly ash based geopolymer concrete
JP2013545714A|2013-12-26|Geopolymer composite for ultra-high performance concrete
CA2658117C|2014-05-13|Geopolymeric cement based on fly ash and harmless to use
EP1507749B1|2011-08-03|Poly|-based geopolymeric cement and production method thereof
CA2420775C|2010-10-26|Highly resistant and ductile fibre concrete
KR20080077002A|2008-08-20|Multi-function composition for settable composite materials and methods of making the composition
WO2012034404A1|2012-03-22|Gypsum whisker, enhanced mineral wool sound-absorbing plate containing the same and preparation method thereof
He et al.2011|Geopolymerization of red mud and fly ash for civil infrastructure applications
FR3005466A1|2014-11-14|HYDRAULIC BINDER COMPOSITION COMPRISING SCORIES AND ASHES
AU2017305533B2|2022-01-27|Dry particulate compositions for the formation of geopolymers, a process for forming geopolymers and the geopolymers obtained as a result
Timakul et al.2015|Effect of silica to alumina ratio on the compressive strength of class C fly ash-based geopolymers
EP3287427A1|2018-02-28|Dry particulate compositions for the formation of geopolymers, a process for forming geopolymers and the geopolymers obtained as a result
CA2305486C|2003-07-29|Aqueous suspension based on alkaline aluminium polysulphate, preparation method and use in the field of building materials
Scanferla et al.2021|The effect of fillers on the fresh and hardened properties of 3D printed geopolymer lattices
Alok et al.2020|Strength studies on Geopolymer Concrete produced by Recycled Coarse Aggregate and Quarry Stone Dust as Fine Aggregate
PL226104B1|2017-06-30|Geopolymer material and method for manufacturing geopolymer material
Kupaei et al.2013|A review on fly ash-based geopolymer concrete
US10800704B2|2020-10-13|Fly ash-based geopolymer concrete and method of formation
Nicoara et al.2019|Alkali Activated Mortars with Intumescent Properties
Nazari et al.2015|Boroaluminosilicate geopolymers: role of NaOH concentration and curing temperature
Abideng et al.2014|Performance evaluation of metakaolin based geopolymer containing parawood ash and oil palm ash blends
Waijarean et al.2014|The effect of SiO2/Al2O3 ratios on the properties of geopolymers prepared from water treatment residue | in the presence of heavy metals
同族专利:
公开号 | 公开日
AU2016223349A1|2017-08-31|
DK3262008T3|2021-03-15|
ES2863499T3|2021-10-11|
US20180022646A1|2018-01-25|
EP3262008A1|2018-01-03|
US10472282B2|2019-11-12|
EP3262008B1|2020-12-16|
AU2016223349B2|2020-01-23|
WO2016135347A1|2016-09-01|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题

US4042137A|1976-04-08|1977-08-16|Thomas Philip Hughes|Municipal refuse collection system|
US4509985A|1984-02-22|1985-04-09|Pyrament Inc.|Early high-strength mineral polymer|
FR2666253B1|1990-09-04|1992-10-30|Davidovits Joseph|PROCESS FOR OBTAINING A GEOPOLYMERIC BINDER FOR STABILIZATION, SOLIDIFICATION AND CONSOLIDATION OF TOXIC WASTE.|
US20120240825A1|2009-09-22|2012-09-27|Uwe Gehrig|Low-Shrinkage Binder System|
US20110132230A1|2009-12-08|2011-06-09|Chan Han|Geopolymer precursor dry mixture, package, processes and methods|
WO2012083255A1|2010-12-17|2012-06-21|The Catholic University Of America|Geopolymer composite for ultra high performance concrete|
US8580029B2|2011-05-31|2013-11-12|King Abdulaziz City Science And Technology|Reduction of carbon dioxide in the manufacturing of composite construction materials|
DE102013001927B4|2013-02-04|2019-01-17|Refratechnik Holding Gmbh|Geopolymer binder system for Feuerbetone, dry Feuetonetonversatz containing the binder system and the use of the offset|
US9919974B2|2013-03-14|2018-03-20|The Catholic University Of America|High-strength geopolymer composite cellular concrete|
WO2014146173A1|2013-03-20|2014-09-25|Halok Pty Ltd|Assessment method|
CN103449744A|2013-08-26|2013-12-18|温州大学|Fly ash based geopolymer and preparation method thereof|CN106810090A|2017-01-06|2017-06-09|哈尔滨工业大学深圳研究生院|A kind of dregs geo-polymer curing materials and preparation method thereof|
CN107417180A|2017-06-09|2017-12-01|佛山科学技术学院|A kind of graphene soil polywater mud and preparation method thereof|
CN107488008B|2017-07-24|2020-02-07|佛山科学技术学院|Halloysite soil cement and preparation method thereof|
US11214520B1|2018-10-18|2022-01-04|TRUce Global, Inc.|Mortar for eco-masonry element|
EP3666743A1|2018-12-10|2020-06-17|Imertech Sas|Geopolymer foam composition|
FI20195370A1|2019-05-06|2020-11-07|Teknologian Tutkimuskeskus Vtt Oy|A method for treating waste material comprising organic components and low and/or intermediate level radioactive agents and a use of a material|
CN110510966B|2019-09-29|2021-12-31|中国建筑第五工程局有限公司|High-strength residue soil baking-free product and preparation method thereof|
CN111056774B|2019-11-28|2021-04-02|浙江大学|Self-curing anti-crack mortar for geopolymer-based ALCboard and preparation method thereof|
CN110981405A|2020-01-03|2020-04-10|福州大学|Method for preparing novel inorganic polymeric material by using tailings|
CN111056783A|2020-01-06|2020-04-24|深圳屹米达环保科技有限公司|Waste concrete geopolymer and preparation method thereof|
CN111533478A|2020-04-01|2020-08-14|武汉工程大学|Preparation method of geopolymer precursor, product, application and connection method thereof|
CN111675511A|2020-06-04|2020-09-18|浙江建设职业技术学院|Geopolymer coating material for rust prevention and corrosion prevention of reinforcing steel bars and manufacturing and using method thereof|
法律状态:
2017-02-23| PLFP| Fee payment|Year of fee payment: 2 |
2018-02-27| PLFP| Fee payment|Year of fee payment: 3 |
2020-02-25| PLFP| Fee payment|Year of fee payment: 5 |
2021-01-01| PLSC| Search report ready|Effective date: 20210101 |
2021-02-23| PLFP| Fee payment|Year of fee payment: 6 |
优先权:
申请号 | 申请日 | 专利标题
EP15290051|2015-02-27|
[返回顶部]