专利摘要:
The invention relates to a method for manufacturing a support for the manufacture of a semiconductor structure based on element III nitrides characterized in that the method comprises the steps of: - forming (100) a layer buffer (20) on a substrate (10), said buffer layer comprising an upper surface layer based on element III nitrides, - depositing (200) a crystalline layer (30) on the buffer layer, said crystalline layer being deposited from silicon atoms so as to cover the entire surface of the element III nitride top layer. The invention also relates to a support obtained by the method and a semiconductor structure based on the support and its manufacturing method.
公开号:FR3031834A1
申请号:FR1550462
申请日:2015-01-21
公开日:2016-07-22
发明作者:Fabrice Semond;Jean Massies;Eric Frayssinet
申请人:Centre National de la Recherche Scientifique CNRS;
IPC主号:
专利说明:

[0001] FIELD OF THE INVENTION The invention relates to a method for manufacturing a semiconductor structure based on element III nitrides and such a semi-conductor structure. conductive. PRESENTATION OF THE PRIOR ART The semiconductor materials based on nitrides of elements III of the periodic table - such as materials based on gallium nitride GaN - occupy an increasingly important place in the fields of electronics. and optoelectronics, especially for the manufacture of light-emitting diodes.
[0002] Existing methods for manufacturing a semiconductor structure based on element III nitrides, such as gallium nitride GaN on a substrate, for example silicon or sapphire, generally result in a significant through-dislocation density associated with unlike the mesh parameter between the host substrate and the element III nitride semiconductor materials. These through dislocations are particularly disadvantageous in the case of semiconductor structures forming light emitting devices based on element III nitride semiconductor materials since the through dislocations increase the leakage currents and deteriorate the luminescence efficiency. of these light emitting devices.
[0003] Three-dimensional epitaxial techniques - such as epitaxial lateral overgrowth (ELO), pendeo-epitaxy from nano-pillars, addition of antisurfactant species, modification of growth conditions have proved their effectiveness in reducing the density of through-dislocations in element III nitride semiconductor materials. The approach used by these techniques to reduce the density of through dislocations consists in initiating a three-dimensional (island) growth mode, and then promoting the coalescence of the islets to obtain a two-dimensional layer of gallium nitride GaN.
[0004] A popular in-situ technique for reducing through-hole dislocation density is to insert an interlayer of silicon nitride SiNx below the GaN layer. More specifically, a silicon nitride SiNx layer is deposited in situ on a nitride layer of element III, then a layer of gallium nitride GaN is deposited on the silicon nitride SiNx layer. This technique has proved to be effective in reducing through-hole dislocation density for conventional c-plan GaN but also for semi-non-polar orientations.
[0005] It is recognized that a surface treatment based on silicon and ammonia leads to the formation of a nano-porous layer of SiNx silicon nitride which acts as a nano-mask for initiating a three-dimensional growth mode of GaN. The growth of GaN is inhibited in the regions where the SiNx silicon nitride is located. On the other hand, the growth occurs in the nano-pores, that is to say in the openings of the nano-mask. The density and the size of these are controlled by the silicon nitride SiNx deposition time and their distribution on the surface is random. For example, the following documents deal with these topics: The article entitled "A New Method of Reducing Dislocation Density in GaN Layer Grown on Sapphire Substrate by MOVPE" by Sakai et al., J. Cryst. Growth, 221, 334 (2000), the article entitled "Anti-Surfactant in III-Nitride Epitaxy - Quantum Dot Formation and Dislocation Termination" by S. Tanaka et al., Jap. J. Appl. Phys., 39, L83 1 (2000), the article "Efficacy of single and double SiNx interlayers on defect reduction in GaN overlayers grown by organometallic vapor-phase epitaxy", by F. Yun et al., J. Appl. Phys., 98, 123502 (2005), the patent application DE10151092 A1, the patent application WO2007 / 133603 A2.
[0006] It has recently been shown that this type of treatment can also lead to the formation of a crystalline structure noted 3112x3112 R300, particularly in the article "Blocking Growth by Electrically Active Subsurface Layer: The Effects of Si as an Antisurfactant in the Growth of GaN ", by T. Markurt et al. Physical Review Letters 110, 036103 (2013). In this article, the crystalline layer is manufactured so as to obtain a partially covered surface, with greater or less uncovered regions that are called "openings" and this layer is called "nanoporous". During the deposition step of the gallium nitride GaN layer, the epitaxial gallium nitride preferentially grows in the apertures of the nanoporous layer so as to form islands. Once the islands are formed, the growth parameters are adjusted so that the gallium nitride GaN develops laterally so as to cover the areas covered by SiNx, and coalesce to form a layer of gallium nitride GaN (3D growth). The growth of the gallium nitride layer is then continued until a desired thickness of gallium nitride GaN (2D growth) is obtained. The coalescence thickness of gallium nitride GaN is defined as the thickness required to obtain a fully coalesced GaN layer after insertion of the SiNx layer. The reader will have understood that the increase in the duration of the surface treatment, and therefore the amount of SiNx deposited, has the effect of increasing the coverage rate of the SiNx layer and thus to reduce the density of nitride islands. of gallium GaN, which makes it possible to reduce the density of through-dislocations. On the other hand, the lower the gallium nitride islet density GaN, the greater the GaN gallium plating thickness required to achieve coalescence. It is therefore particularly advantageous to determine the optimum coverage rate of the SiNx layer to make such a process exploitable industrially. In addition, the existing processes for manufacturing GaN-based devices on a substrate generally comprise a first step of depositing a buffer layer, which may be, for example, aluminum nitride AIN for a silicum substrate, optionally followed by a deposition step of a layer of AlGaN aluminum and gallium nitride on the aluminum nitride buffer layer AlN. The nano-mask can then be deposited on the AlN or AlGaN layer. Other methods include using a sapphire substrate and depositing a layer of GaN at a low temperature as a buffer layer, in which case the nano-mask is deposited on the GaN buffer layer. A disadvantage of the growth technique with the nano-mask of SiNx mentioned relates to the fact that oxidation reactions can take place on the surface of the buffer layer not covered by the SiNx layer. In particular, the buffer layer can oxidize at the openings in the event of exposure to air of the substrate consisting of the substrate, the buffer layer and the SiNx layer. Therefore, in the methods of the state of the art, the upper (or final) GaN nitride layer is formed on the SiNx layer immediately after the formation thereof, with no possibility of storage of the support prior to deposition. a layer of gallium nitride thereon. Another disadvantage of this technique is that there is no way to define the optimal duration of the deposition step of the nanoporous SiNx layer. This optimal duration, related to the size of the openings and their density, varies according to the starting substrate used for growth, the type of reactor used for growth, and other parameters such as concentrations of gaseous precursors, etc. The size of the openings and their density are non-measurable quantities, therefore the determination of the optimal duration of the deposition step of the nanoporous layer of SiNx can only be obtained empirically by carrying out successive tests which must be repeated at whenever one of the growth parameters (ie substrate, reactor, etc.) is modified, which is costly in time and, above all, does not make it possible to carry out a generic process, that is to say generally applicable . An object of the present invention is to provide a method for overcoming at least one of the aforementioned drawbacks.
[0007] SUMMARY OF THE INVENTION To this end, the invention proposes a method of manufacturing a support for the manufacture of a semiconductor structure based on nitrides of elements III, characterized in that the method comprises the steps of: forming a buffer layer on a substrate, said buffer layer comprising an upper layer based on nitrides of elements III, depositing a crystalline layer on the buffer layer, said crystalline layer being deposited from atoms of silicon so as to cover the entire surface of the III-nitride-based top layer, said crystalline layer having a triple periodicity of silicon atoms in the crystallographic direction [1-100] so that an image diffraction of said crystalline layer obtained by electron diffraction grazing incidence in the direction [1-100] comprises: - a central line (0, 0) and lines of integer order (0, -1) and (0 , 1), - two diffraction lines of non-integer order (0, -1/3) and (0, -2/3) between the central line (0, 0) and the integer line (0, -1), and - two non-integer (0, 1/3) and (0, 2/3) diffraction lines between the central line (0, 0) and the integer line (0, 1).
[0008] Depositing a crystalline layer which covers the entire surface of the buffer layer on the substrate allows the surface of the buffer layer to be completely passivated and thus to prevent any oxidation reaction thereof. This makes it possible to store the support composed of the substrate, the buffer layer and the crystalline layer prior to the deposition of the semiconductor structure based on element III nitrides. The step of depositing a crystalline layer that covers the entire surface also makes it possible to dispense with the empirical phases of development and optimization of the processes of the prior art based on a deposition step of a nanoporous layer of SiNx, in particular the determination of the optimum size of the nanopores as well as the optimum density of the nanopores. The deposition step of a silicon-based crystalline layer further allows for subsequent growth of an III-based nitride layer thereon, whereas a nanoporous amorphous layer overlying the base-based top layer nitride III would not allow this further growth. The diffraction pattern described corresponds to a hexagonal periodic arrangement rotated 30 ° with respect to the network of the element III nitride-based layer and with a mesh parameter V times greater than the mesh parameter of the network of the layer. based on element III nitride, which promotes this subsequent growth of a crystalline layer.
[0009] It will be understood in the following that when a layer A is mentioned as being on a layer B, it may be directly on the layer B, or may be located above the layer B and separated from said layer B by one or more intermediate layers.
[0010] It will also be understood that when a layer A is mentioned as being on a layer B, it may cover the entire surface of the layer B, or a portion of said layer B. Preferred but nonlimiting aspects of the device according to the invention. The invention is as follows: the crystalline layer has a simple periodicity in the crystallographic direction [1-210] so that a diffraction image of said crystalline layer obtained by grazing incidence diffraction of electrons in the direction [1-10]; 210] comprises a central line (0, 0) and lines of integer order (0, -1) and (0, 1) zo without lines of non-integer order between them; the substrate is based on silicon and the step of forming the buffer layer includes the deposition of a layer of aluminum nitride AlN forming the upper surface layer based on element III nitrides; the substrate is based on silicon and the step of forming the buffer layer includes the deposition of a layer of aluminum nitride AlN and the deposition of a layer of gallium nitride layer and AlGaN aluminum forming the upper surface layer based on III element nitrides on the aluminum nitride AlN layer; the buffer layer has, at the end of its formation, a thickness of between 10 and 200 nm; the deposition step of the semi-crystalline layer consists of a deposit under ultra-vacuum; the deposition step of the semicrystalline layer consists of a deposition by molecular beam epitaxy; the method comprises a step of measuring the crystalline layer by electron diffraction grazing incidence in the crystallographic direction [1-100] during the deposition step of the crystalline layer so as to obtain a diffraction image of said layer crystalline, and the duration of the step of depositing the crystalline layer is a function of the intensity of at least one diffraction line of the diffraction pattern of the crystalline layer in the crystallographic direction [1-100]; the diffraction pattern of the crystalline layer in the crystallographic direction [1-100] comprises: - a central line (0, 0) and lines of integer order (0, -1) and (0, 1), - two diffraction lines of non-integer order (0, -1/3) and (0, -2/3) between the central line (0, 0) and the line of integer order (0, -1) and two non-integer (0, 1/3) and (0, 2/3) diffraction lines between the central line (0, 0) and the integer line (0, 1). the step of depositing the crystalline layer being interrupted when the luminous intensity of said non-integer order lines is maximum; the deposition step of the semicrystalline layer consists of a vapor phase deposition; the step of depositing the semicrystalline layer consists of an organometallic vapor phase epitaxy deposit; The crystalline layer is deposited from silicon atoms and ammonia molecules. The invention also relates to a support for the manufacture of a semiconductor structure based on element III nitrides, characterized in that it comprises: - a substrate, - a buffer layer on the substrate, the buffer layer comprising a upper layer based on III element nitrides, - a crystalline layer on the buffer layer, said crystalline layer including silicon atoms and covering the entire surface of the upper layer based on nitrides III elements of the buffer layer, said crystalline layer having a triple periodicity of silicon atoms in the [1-100] direction, such that a diffraction pattern of said crystalline layer obtained by electron diffraction in grazing incidence in the direction [1 -100] comprises: - a central line (0, 0) and lines of integer order (0, -1) and (0, 1), - two diffraction lines of non-integer order (0, -1 / 3) and (0, -2/3) between the central line (0, 0) and the line of integer order (0, -1), and - two diffraction lines of non-integer order (0, 1/3) and (0, 2/3) between the central line (0, 0) and the line of integer order (0, 1).
[0011] Preferred but non-limiting aspects of the support according to the invention are the following: the crystalline layer has a simple periodicity in the crystallographic direction [1-210] so that a diffraction image of said crystalline layer obtained by diffraction of electrons at grazing incidence in the direction [1-210] has a central line (0, 0) and lines of integer order (0, -1) and (0, 1) without any non-integer order lines between those -this ; the substrate is based on sapphire A1203, silicon Si, silicon on insulator SOI, silicon carbide SiC, aluminum nitride AlN, zinc oxide ZnO or gallium arsenide GaAs; the substrate is based on silicon and the buffer layer comprises a layer of aluminum nitride AIN and a layer of gallium aluminum nitride AlGaN on the layer of aluminum nitride AIN; the crystalline layer has a thickness of between 2 A and 6 A; The buffer layer has a thickness of between 10 and 200 nm. The invention also relates to a method of manufacturing a semiconductor structure based on element III nitrides, comprising the steps of: - providing a support according to the invention, - growth of a semiconductor structure based on of nitrides of elements III on the crystalline layer. Preferably, the growth step comprises a step of depositing a layer of gallium nitride GaN on the crystalline layer. Preferably, the growth step consists of organometallic vapor phase deposition. The invention also relates to a semiconductor structure based on element III nitrides, comprising: - a support according to the invention, - a semiconductor material based on element III nitrides on the crystalline layer. Preferably, the element III nitride semiconductor material on the crystalline layer comprises a layer of gallium nitride. Gallium nitride GaN has a through dislocation density of less than or equal to 5 × 10 8 cm -2. Preferably, the element III nitride semiconductor material on the crystalline layer comprises an aluminum-based layer.
[0012] The invention also relates to a light-emitting diode based on nitrides of elements III, characterized in that it comprises - a semiconductor structure according to the invention, - a first contact layer based on gallium nitride disposed on the first nitride-based semiconductor layer III, - a second gallium-nitride contact layer disposed on the first gallium-nitride contact layer, - an active layer having a structure multiple quantum well arrangement disposed between the first gallium nitride contact layer and the second gallium nitride contact layer.
[0013] BRIEF DESCRIPTION OF THE DRAWINGS Other advantages and characteristics of the process according to the invention and of the associated product will become more apparent from the following description of several variant embodiments, given by way of non-limiting examples, from the accompanying drawings on which: - Figure 1 illustrates an example of a method of manufacturing a semiconductor structure based on element III nitrides; FIG. 2 schematically illustrates an example of a product obtained by implementing the method illustrated in FIG. 1; FIGS. 3 and 4 illustrate two diffraction images in the crystallographic directions [1-100] and [1-210], respectively, a crystalline layer according to the invention; - Figure 5 illustrates a semiconductor structure having a mesa structure; - Figure 6 illustrates a semiconductor structure having a box structure.
[0014] In the different figures, the same references designate similar elements. DETAILED DESCRIPTION OF THE INVENTION The process according to the invention will now be described in more detail with reference to the growth of a GaN gallium nitride layer on a support, enabling the production of light-emitting diodes. The nitride-based layer of elements III can be a thick layer ("template" in English) or self-supported, also called bulk substrate ("bulk substrate" in English). The semiconductor structure based on nitride of elements III can thus be a GaN, AlN, etc thick layer, or a solid GaN, AlN, etc. substrate, or else an epitaxial structure (epiwafer in English). . However, it is obvious to those skilled in the art that the process described hereinafter can be used to grow an element III nitride material other than gallium nitride, which material can be used to carry out other semiconductor structures than light-emitting diodes. For example, the resulting structure may thus have a light emitting diode configuration, or a high electron mobility transistor (HEMT). FIG. 1 illustrates an alternative embodiment of the method according to the invention. The method comprises the steps of: forming a buffer layer on a substrate, said buffer layer comprising an element-nitride top surface layer; depositing a crystalline layer on the buffer layer; growing 300 a layer of gallium nitride on the crystalline layer, said crystalline layer being deposited from silicon atoms.
[0015] Substrate To manufacture the semiconductor structure, a substrate 10 is used on which 5 different deposition steps are carried out. The substrate 10 used may be sapphire Al 2 O 3, silicon Si, silicon carbide SiC, aluminum nitride AlN, zinc oxide ZnO or gallium arsenide GaAs. In one embodiment, the substrate is silicon. The use of a silicon substrate has many advantages over the use of a sapphire substrate; in particular: a silicon substrate is less expensive than a sapphire substrate; the dimensions of the silicon substrates (generally up to 12 inches, or 30.48 cm) are larger than those of the sapphire substrates (generally up to 6 inches, or 15.24 cm); it is therefore possible to manufacture a GaN gallium nitride layer of larger surface area using a silicon substrate; the different stages of manufacture of the post-growth components (backside polishing, front face transfer, removal of the substrate, etc.) after the growth of the gallium nitride GaN layer are simpler and less costly in the case of use of a silicon substrate only in the case of a sapphire substrate. Thus, the use of silicon substrates makes it possible, for example, to manufacture light-emitting diodes (LEDs) at low production cost, which can be particularly advantageous in the field of lighting. Advantageously, the substrate 10 may be a patterned substrate comprising a mesa structure 11 in the form of a raised tray (the size of which may vary from 10x10 μm to 400x400 μm) and obtained by etching the surface of the substrate surrounding the tray. , as illustrated in FIG. 5, or else a box structure, as represented in FIG. 6, in which the buffer layer 20 based on element III nitride, in this case AlN and AlGaN, the crystalline layer. 30 covering it completely and the gallium nitride layer 40 are located in a recess 12 formed in the substrate 10. Another method of manufacturing the patterns, such as for example the partial masking of the surface by a mask made of dielectric materials, may be advantageously used. The use of such a patterned substrate makes it possible to limit the cracking of the layer of gallium nitride epitaxialized on the substrate 10, and thus to increase the critical thickness of gallium nitride GaN that can be deposited on the substrate 10 without creating cracks. For example, it is possible to produce an uncracked layer of GaN gallium nitride of thickness 5 μm using a substrate including a mesa structure of 200 × 200 μm, whereas the use of an unstructured substrate makes it possible to achieve only uncracked layer of gallium nitride GaN 1 μm thick. Buffer layer formation The method comprises a step 100 of forming a buffer layer 20 comprising an upper surface layer based on element III nitrides. This buffer layer may for example comprise a layer of aluminum nitride AlN, AlGaN aluminum gallium nitride, AlGaBN aluminum-aluminum boron nitride, an AlN / AlGaN stack, a AlGaN gradual, AlGaN oxide, AlGaN zinc ZnO, or BN boron nitride or silicon carbide SiC. However, in all cases, the buffer layer has a top layer of element III nitrides, such as aluminum nitride AlN, AlGaN aluminum gallium nitride. In the case of the example of the present description, this forming step 100 comprises the deposition 110 of a layer 21 of aluminum nitride AIN on the substrate 10. This layer 21 of aluminum nitride AlN may constitute the upper surface layer based on element III nitrides of the buffer layer 20. The formation of a buffer layer 20 including a layer 21 of aluminum nitride AIN improves the quality of the nitride layer 40 gallium GAN subsequently deposited.
[0016] For example, when the substrate 10 used is silicon Si, the direct growth of gallium nitride GaN on silicon Si is very difficult, particularly because of the high chemical reactivity between gallium Ga, silicon Si at high temperature. The formation of a buffer layer 20 including a layer 21 of aluminum nitride AIN makes it possible to overcome these difficulties, and therefore to improve the quality of the layer 40 of gallium nitride GaN epitaxially grown. The buffer layer 20 may have a thickness between 10 nm and 500 nm, preferably between 10 pm and 200 nm. A buffer layer with a thickness greater than 200 nm makes it possible to obtain a good crystalline quality of the buffer layer 20, and therefore to improve that of the epitaxially-grown III nitride layer. The crystalline layer according to the invention, which completely covers the buffer layer, however, makes it possible to ensure good crystalline quality of the epitaxially-enriched III-nitride layer, even if the crystalline quality of the buffer layer is not maximal. . Therefore, it is not necessary for the buffer layer 20 to reach a thickness greater than 200 nm. Thus, preferably, the buffer layer 20 has a thickness of between 10 and 200 nm, or even between 50 and 100 nm. The fact of limiting the thickness of the buffer layer 20 to below 200 nm advantageously makes it possible to reduce the duration of the process, since the growth time of a layer 21 of aluminum nitride AIN is relatively long. Another advantage is that with a thin buffer layer 20, which is completely covered by a crystalline layer, the problem of dislocations in this buffer layer solved by the crystalline layer 30 is all the more quickly resolved, preventing dislocations from spreading and causing dislocations.
[0017] The forming step 100 of the buffer layer 20 may also comprise an optional step 120 of depositing a layer 22 of aluminum nitride and gallium AlGaN on the aluminum nitride layer 21 AIN. This layer 22 of aluminum nitride and gallium AlGaN then forms the upper surface layer based on element III nitride of the buffer layer 20. This makes it possible to obtain a complex buffer layer 20 of aluminum nitride AIN and of AlGaN aluminum and gallium nitride.
[0018] The layer 22 of AlGaN aluminum gallium nitride makes it possible to reduce the dislocation density of the layer on which the crystalline layer is deposited. Advantageously, the thickness of the buffer layer, and therefore the sum of the thicknesses of the layers 21, 22 of aluminum nitride AIN and of aluminum and gallium AlGaN nitride can be between 10 nm and 500 nm, preferably between 50 and 200 nm with, for example, the following distribution: 25-100 nm of aluminum nitride AlN, 25-400 nm of AlGaN aluminum gallium nitride.
[0019] This makes it possible to reduce the growth time of the buffer layer while benefiting from the advantages relating to the deposition of aluminum nitride and aluminum and gallium nitride layers.
[0020] Preferably, the surface of the buffer layer, i.e., the surface of the element III nitride layer on which the crystalline layer will be deposited, is formed as smooth as possible. Deposition of a Crystalline Layer The process also comprises a step of deposition 200 of a crystalline layer 30 on the buffer layer 20. The crystalline layer is deposited from a precursor containing silicon Si atoms. The precursor containing atoms silicon can for example be silane SiH4, disilane Si2H6, or timethylsilane SiH (CH3) 3. The deposition can also be carried out by exposing the surface of the buffer layer 20 to Si silicon atoms and NH 3 ammonia molecules.
[0021] The crystalline layer 30 is deposited in such a way as to cover the entire surface of the buffer layer 20 constituted by the upper surface of the nitride-based layer III, for example the aluminum nitride layer 21 or the layer 22 of gallium nitride.
[0022] The step of depositing the crystalline layer 30 corresponds to a surface treatment which leads to a surface reconstruction of the atoms deposited on the surface of the buffer layer 20. In fact, following the exposure of the surface of the buffer layer At the silicon Si atoms and optionally at the NH 3 ammonia molecules, silicon Si atoms bind to the surface of the buffer layer creating a hexagonal arrangement rotated 30 ° with respect to the network of the nitride layer. of elements III on which the atoms are deposited and with a mesh parameter times greater than that of the nitride layer of elements III. The formation of this surface reconstruction is measurable by electron diffraction techniques and its coverage rate of the surface can be quantified by recording the intensity of diffraction lines specific to this surface reconstruction. Electron diffraction is a technique used for the study of matter which involves bombarding a sample with electrons and observing the resulting diffraction pattern. An example of an electron diffraction technique that can be used in the context of the present invention to study the structure of the crystalline layer is the high energy electron diffraction (RHEED) diffraction. is a technique for determining the crystalline structure of the surface in an ultra-empty environment. In particular, the RHEED technique makes it possible to determine the reconstruction of the surface, to measure the speed of growth and to qualitatively assess the flatness of the surface. A RHEED device consists of an electron gun that creates a monocinetic electron beam with an energy of 10 to 50 keV focused on the surface. The wavelength associated with the electrons is of the order of 0.1 A. The beam reaches the grazing incidence surface at an angle of 1 to 2 degrees. In this configuration the interaction of electrons with the surface is limited to a few atomic planes. The electrons reflected and diffracted by the atoms of the surface are collected on a fluorescent screen which makes it possible to visualize the corresponding diffraction pattern and this photograph can then be digitized using a CCD camera. The document "Reflection High Energy Electron Diffraction", by Ayahiko Lchimiya and Philip I. Cohen, Cambridge University Press, 2004, describes this technique. With reference to FIGS. 3 and 4, two diffraction images of the crystalline layer are illustrated in the respective crystallographic directions [1-100] and [1-210].
[0023] In FIG. 4, the diffraction pattern of the crystalline layer in the direction [1210] comprises only whole-order diffraction lines: a central line (0.0) 42 and two integer lines (0, -1) 43 and (0, 1) 44 on either side of said central line 42. Thus there are no lines of non-integer order between the lines of integer order (0, -1 ) and (0, 1) and the central line (0, 0). It should be noted that the spacing between whole-order diffraction lines is inversely proportional to the mesh parameter in the plane of the surface. In FIG. 3, however, corresponding to the diffraction pattern of the crystalline layer in the [1-100] direction, the presence of a surface reconstruction leads to the presence of additional fractional lines. that is to say of non-integer order, in this case of 1/3 order characteristic of a reconstruction called 1x3. The diffraction pattern of the crystalline layer in the [1-100] direction thus comprises: - a central line (0, 0) and lines of integer order (0, -1) and (0, 1), - two non-integer order diffraction lines 31, say (0, -1 / 3) and (0, -2/3), between the lines (0, 0) 32 and (0, -1) 33, and two non-integer order diffraction lines 35, say (0, 1/3) and (0, 2/3), between the lines (0, 0) 32 and (0, 1) 34. Therefore, the diffraction pattern in the [1-210] direction having only a space between the whole order lines, whereas the diffraction pattern in the [1-100] direction having three spaces between the lines of entire order, that is why this crystalline layer is called 1x3.
[0024] Thus, and contrary to the methods of the prior art comprising a step of deposition of a nanoporous SiNx layer whose structure and exact composition are unknown, the method according to the invention proposes the deposition of a crystalline layer called 1x3 of structure and composition perfectly defined, and whose pore density is preferably the lowest possible, or substantially zero. In fact, in the methods of the state of the art, it is sought to avoid a total coverage rate of the surface of the nitride-based layer III. However, the inventors have discovered that the dislocation density is minimal when the zo crystalline layer covers the entire surface of the element III nitride-based layer. It should be noted that the 1x3 crystalline layer may have a very small thickness, of the order of the monolayer of silicon atoms, of the order of 2 to 3 A. In fact, in order to preserve the crystalline character of the 1x3 crystalline layer, the thickness thereof is preferably less than 6 A. Advantageously, the deposition of the 1x3 crystalline layer induces a passivation of the surface of the buffer layer. This passivation makes it possible to render the buffer layer 30 inert with respect to exposure to air and thus to prevent any oxidation reaction. Obtaining a support for the growth of gallium nitride GaN At the end of the deposition step 200 of the crystalline layer 30, a support is obtained for the growth of a semiconducting structure based on nitrides. elements III, such as a layer of gallium nitride GaN.
[0025] This support comprises: a substrate 10 chosen from the group consisting of silicon Si, silicon carbide SiC, aluminum nitride AlN, zinc oxide ZnO, sapphire or gallium arsenide GaAs; a buffer layer comprising an upper layer based on nitrides of elements III, which may for example have a thickness of between 100 μm and 200 μm; a crystalline layer 30 whose thickness may be between 2 and 6 A, preferably between 2 and 3 A.
[0026] Growth of a Gallium Nitride Layer The process also comprises a step of growing a semiconductor structure based on element III nitrides, such as the growth of a layer of gallium nitride, on the crystalline layer 30.
[0027] The principle of growth of the GaN gallium nitride layer on the 1x3 crystal layer is as follows. The deposition of the 1x3 crystal layer makes it possible to increase the diffusion length (i.e. diffusion amplitude characterizing the interaction of a neutron with a given isotope) of the species deposited on the crystalline layer. The crystalline layer forms a surface that is energetically unfavorable to the growth of nitrides III. This anti-surfactant effect induces the formation of islets whose size and shape are determined by the surface energy of the crystalline layer, and by the kinetics of growth. During the deposition step of the gallium nitride GaN layer, the gallium nitride GaN develops laterally from the islands, forming by coalescence a layer of gallium nitride GaN (3D growth). The growth of the gallium nitride layer is then continued until a desired thickness of gallium nitride GaN (2D growth) is obtained.
[0028] A layer stack composed of a substrate, a buffer layer, a crystalline layer and a gallium nitride layer is then obtained. The density of through-dislocations that emerge at the surface can be measured by transmission electron microscopy (TEM or TEM) for transmission electron microscopy. The density of traversing dislocations is less than or equal to 5 × 10 8 cm -2. The gallium nitride GaN therefore has a reduced through-dislocation density compared to a GaN layer formed according to a method of the state of the art, without the 1x3 crystalline layer.
[0029] It is found that the zone of coalescence in the layer of gallium nitride, at which dislocation coalescences are observed, extends to a thickness of less than 2 μm from the surface of the crystalline strain 30, as it can be observed by observation under the electron microscope.
[0030] The coalescence thickness of gallium nitride GaN is defined as the thickness required to obtain a fully coalesced GaN layer, i.e. having a continuous layer plane, above the surface after insertion. of the crystalline layer. We can no longer distinguish there islets.
[0031] Of course, the gallium nitride GaN layer can then be separated from the substrate and the buffer layer, for example to obtain a layer of gallium nitride GaN self-supported. Growth techniques used Advantageously, the steps of: - formation of the buffer layer 20, and / or deposition of the crystalline layer 30 on the buffer layer 20, can be carried out by ultra-vacuum deposition, preferably by epitaxy by molecular jets EJM (or "MBE" acronym of the English expression "molecular beam epitaxy").
[0032] It is also possible that the step of depositing the crystalline layer 30 and / or the buffer layer 20 consists of a vapor phase deposition, more specifically a vapor deposition epitaxial vapor with organometallic EPVOM (or "MOVPE" acronym of the English expression "Metalorganic vapor phase epitaxy").
[0033] The fact of forming the buffer layer by molecular beam epitaxy - and therefore in an ultrahigh vacuum environment - has many advantages over organometallic vapor phase epitaxy buffer layer formation techniques.
[0034] In particular, the formation of the buffer layer 20 by molecular beam epitaxy allows: on the one hand to eliminate any trace of reactive gas in the environment of the substrate once the buffer layer 20 has been formed, and thus to limit the risks of parasitic reaction nitriding the surface of the substrate, - secondly to limit the fouling of the growth reactor and thus improve the manufacturing efficiency by reducing the frequency of maintenance operations of the reactor. In addition, the formation of the buffer layer 20 by molecular beam epitaxy provides a very smooth surface of the element III nitride layer, thereby improving the formation of the crystalline layer 30. In addition, the use of ultravide in EJM also allows in-situ monitoring - for example by electron diffraction - of the deposition of the crystalline layer. This allows precise monitoring of the deposition step of the crystalline layer so as to stop this step when the thickness of the crystalline layer totally covers the surface.
[0035] Thus, the method may comprise a step of measuring the coverage rate of the crystalline layer by graft incidence electron diffraction in the [1-100] direction during the crystalline layer deposition step 30 so as to obtain a diffraction pattern of said crystalline layer 30, wherein the duration of the crystalline layer deposition step is a function of the intensity of at least one non-integer diffraction line of a diffraction pattern of the crystalline layer obtained by electron diffraction in the crystallographic direction [1-100].
[0036] As indicated above, the diffraction pattern of the crystalline layer 30 in the [1-100] direction then comprises: - a central line (0, 0) and lines of integer order (0, -1) and (0 , 1), - two non-integer (0, -1/3) and (0, -2/3) diffraction lines between the central line (0, 0) and the whole order line (0 , -1), and - two diffraction lines of non-integer order (0, 1/3) and (0, 2/3) between the central line (0, 0) and the integer line (0 , 1). Preferably, the step of depositing the crystalline layer 30 is interrupted when the luminous intensity of the non-integer order intermediate lines of the diffraction pattern (in the crystallographic direction [1-100]) is maximum; which corresponds to a complete coverage rate of the surface of the element III nitride layer by the crystalline layer 30. This maximum intensity is easily identifiable. In fact, by using a CCD camera, it is sufficient to record the intensity profile of one of the non-integer order diffraction lines in the direction [1-100] as a function of the deposition time of the film layer. passivation. At first, the diffraction line of non-integer order appears then its intensity increases during the deposition, to arrive at a step before in a second time to decrease and not to disappear. The maximum intensity is therefore detectable by the stability of this intensity, which can last several minutes. Similarly, the growth step of the semiconductor structure - such as a layer of gallium nitride - can be carried out by a vapor deposition such as by EPVOM.
[0037] Example of a Manufacturing Process An example of a method according to the invention will now be described. The aim here is to produce a thin layer of gallium nitride GaN on a silicon Si substrate, the gallium nitride layer GAN having a low dislocation density (TDD <5.108 cm-2, where "TDD" is the acronym for the Anglo-Saxon term "Threading Dislocation Density"). The silicon substrate used has a crystallographic orientation (111). An aluminum nitride buffer layer is formed on the silicon substrate by molecular beam epitaxy. The formation of the buffer layer is interrupted when the thickness thereof is between 10 and 200 nm. The step of depositing the 1x3 crystalline layer is then carried out. A treatment of the surface of the buffer layer by molecular beam epitaxy is carried out using silicon atoms and NH 3 ammonia molecules. This surface treatment leads to the formation of a new crystal structure that is well defined, measurable and identifiable by electron diffraction. During deposition of the crystalline layer, the surface is observed by an electron diffraction technique of grazing incidence delivery of a monocinetic electron beam onto the crystalline layer being formed to observe the resulting diffraction pattern ( following the crystallographic direction [1100]). The ordered periodic structure of the 1x3 crystal layer makes it possible to diffract the electrons and thus obtain a specific diffraction image. The duration of the deposition step of the crystalline layer is a function of the intensity of at least one non-integer diffraction line observed on the diffraction image. In particular, the step of depositing the crystalline layer is interrupted when the intensity of at least one of the diffraction lines observed in the diffraction pattern is maximum, which is detectable by the stability of this intensity.
[0038] The GaN gallium nitride layer is then grown. The crystalline layer makes it possible to initiate a 3D growth mode of gallium nitride GaN. Islands of gallium nitride GaN form on the surface of the crystalline layer. The islands of gallium nitride GaN enlarge and eventually form a coalesced layer after about 2 microns.
[0039] A GaN gallium nitride layer with a thickness of 2 μm and a dislocation density of less than 4.108 cm-2 is thus obtained. Examples of gallium nitride layers obtained by other methods are given as an indication in the following table. (Growth technique) Substrate Thickness GaN Density Dislocations (cm-2) Width mid-height (Pm) (002) (102) 2 Invention Si (111) - 4x10 ^ 8 439C 468 "(200nmAIN) (EJM + EPV0M) 1.5 450570" OSRAM (AlN / AlGaN (EPVOM) S (111) 400 nm)> 8x10''8 1.7 533 "- IMEC (AlN / AlGaN (EPVOM) Si (111) 1.5 mm) -3 × 10 -8 700 1050 "Korea PTI (EPVOM) S (111) 1 2x10 ^ 9 Singapore MIT (EPVOM) Si (111) 2.2 - 101 9 - - Si (111)> 4 U. Magdeburg (EPVOM) - 1x10 ^ 9 240" 300 "Univ. Virginia (EPVOM) 6H-S C 8 4x10 ^ 8 185 "325" U. Cambridge (EPVOM) Sapphire 3 - 2x10 ^ 8 U. Cambridge 175 "170" (EPVOM) Sapphire 12 - 5x10 ^ 7 205 "221" Univ. Virginia (EPVOM) Sapphire 6 - 3,5x10 ^ 7,305 "415" Lumilog (EPVOM) Sapphire 4 5x10 ^ 8,240 "315" Lumilog (EPVOM) Sapphire 9 - 8x10 ^ 7 As can be seen from the table above the existing processes using a silicon substrate for the growth of a gallium nitride layer do not make it possible to obtain a layer of gallium nitride of equivalent quality to the process according to the invention. Furthermore, it can be seen that even if the processes using a sapphire substrate for the growth of a gallium nitride layer make it possible to obtain a layer of gallium nitride having a dislocation density equivalent to the process according to the invention, the The thickness of the epitaxial GaN gallium nitride layers is greater. It will be understood by those skilled in the art that many modifications can be made to the process described above without materially going out of the new teachings presented here. For example, the steps of forming the buffer layer and depositing the crystalline layer can be performed by EPVOM. On the other hand, the growth step of the element III nitride semiconductor structure can be carried out by EJM. It is possible to obtain a nitride electroluminescent diode of element III nitride elements, comprising a semiconductor structure previously described, a first contact layer based on gallium nitride disposed on the first layer. III nitride semiconductor material, - a second gallium nitride contact layer disposed on the first gallium nitride contact layer, - an active layer having a structure of multiple quantum well disposed between the first gallium nitride contact layer and the second gallium nitride contact layer. It is therefore obvious that the examples which have just been given are only particular illustrations which are in no way limiting.
权利要求:
Claims (26)
[0001]
REVENDICATIONS1. A process for manufacturing a support for the manufacture of a semiconductor structure based on nitrides of elements III characterized in that the method 5 comprises the steps of: - forming (100) a buffer layer (20) on a substrate (10), said buffer layer comprising an upper layer based on element nitrides; - depositing (200) a crystalline layer (30) on the buffer layer, said crystalline layer being deposited from atoms of silicon so as to cover all of the surface of the element III nitride top layer, said crystalline layer (30) having a triple periodicity of silicon atoms in the crystallographic direction [1-100] so that a diffraction pattern of said crystalline layer obtained by graft incidence electron diffraction in the [1-100] direction comprises: - a center line (0, 0) and whole order lines (0, - 1) and (0, 1), - two lines of non-integer (0, -1/3) and (0, -2/3) order diffraction between the central line (0, 0) and the integer line (0, -1), and - two non-integer (0, 1/3) and (0, 2/3) order diffraction lines between center line (0, 0) and integer line (0, 1). 20
[0002]
2. The method of claim 1, wherein the crystalline layer has a simple periodicity in the crystallographic direction [1-210] so that a diffraction image of said crystalline layer obtained by electron diffraction grazing incidence in the direction [1-210] has a central line (0, 0) and lines of integer order (0, -1) and (0, 1) without any non-integer order lines therebetween.
[0003]
3. Method according to one of the preceding claims, wherein the substrate is based on silicon and the forming step (100) of the buffer layer (20) includes the deposition (110) of a nitride layer. AIN aluminum (21) forming the upper surface layer based on element III nitrides.
[0004]
The method according to one of claims 1 or 2, wherein the substrate is silicon-based and the step (100) of forming the buffer layer (20) includes - depositing (110) a layer of aluminum nitride AIN (21) and 27 3031834 - the deposition (120) of a layer a layer of aluminum gallium nitride AlGaN (22) forming the upper surface layer based on element III nitrides on the aluminum nitride layer AIN (21).
[0005]
5. Method according to one of the preceding claims, wherein the buffer layer (20) has, at the end of its formation, a thickness between 10 and 200 nm.
[0006]
6. Method according to one of the preceding claims, wherein the step of depositing the semi-crystalline layer consists of a deposit under ultra-vacuum, preferably a deposit by molecular beam epitaxy.
[0007]
7. Method according to the preceding claim, comprising a step of measuring the crystalline layer by electron diffraction grazing incidence in the crystalline plane [1-100] during the deposition step of the crystalline layer so as to obtain an image diffraction of said crystalline layer, and the duration of the deposition step of the crystalline layer (30) is a function of the intensity of at least one non-integer diffraction line of the diffraction pattern of the crystalline layer in the crystallographic direction [1-100].
[0008]
8. Method according to the preceding claim, wherein the diffraction pattern of the crystal layer in the direction [1-100] comprises: - a central line (0, 0) and lines of integer order (0, -1) ) and (0, 1), two diffraction lines of non-integer order (0, -1/3) and (0, -2/3) between the central line (0, 0) and the line of integer order (0, -1), and - two diffraction lines of non-integer order (0, 1/3) and (0, 2/3) between the central line (0, 0) and the line of integer order (0, 1). the step of depositing the crystalline layer being interrupted when the light intensity of said non-integer order lines is maximum.
[0009]
9. Method according to one of the preceding claims, wherein the crystalline layer has a thickness between 2 and 6 A. 28 3031834
[0010]
The process of claim 1, wherein the step of depositing the semicrystalline layer is a vapor deposition.
[0011]
11. Process according to the preceding claim, in which the step of depositing the semicrystalline layer consists of an organometallic vapor phase deposition.
[0012]
12. A process according to any one of the preceding claims, wherein the crystalline layer is deposited from silicon atoms and ammonia molecules.
[0013]
13. Support for the manufacture of a semiconductor structure based on element III nitrides, characterized in that it comprises: - a substrate (10), - a buffer layer (20) on the substrate, the buffer layer comprising an upper layer based on element III nitrides, - a crystalline layer (30) on the buffer layer, said crystalline layer including silicon atoms and covering the entire surface of the nitride-based top layer of the buffer layer elements III, said crystalline layer (30) having a triple periodicity of silicon atoms in the [1-100] direction, such that a diffraction pattern of said crystalline layer obtained by diffraction of electrons at grazing incidence in the direction [1-100] comprises: - a central line (0, 0) and lines of integer order (0, -1) and (0, 1), - two diffraction lines of non-integer order (0, -1/3) and (0, -2/3) between the central stripe (0, 0) and the stripe e of integer order (0, -1), and - two diffraction lines of non-integer order (0, 1/3) and (0, 2/3) between the central line (0, 0) and the integer line (0, 1). 30
[0014]
14. Support according to the preceding claim, wherein the crystalline layer has a simple periodicity in the crystallographic direction [1-210] so that a diffraction image of said crystalline layer obtained by electron diffraction incidence grazing in the direction [1-210] has a central line (0, 0) and lines of integer order (0, -1) and (0, 1) without any non-integer order lines therebetween.
[0015]
15. Support according to any one of claims 13 to 14, wherein the substrate (10) is based on sapphire A1203, silicon Si, silicon on insulator SOI, silicon carbide SiC, aluminum nitride AIN, zinc oxide ZnO or gallium arsenide GaAs.
[0016]
16. Support according to any one of claims 13 to 14, wherein the substrate (10) is silicon-based and the buffer layer comprises a layer of aluminum nitride AlN (21) and a layer of gallium nitride and AlGaN aluminum (22) on the aluminum nitride AlN layer (21).
[0017]
17. Support according to one of claims 13 to 16, wherein the crystalline layer 15 has a thickness between 2 A and 6 A.
[0018]
18. Support according to one of claims 13 to 17, wherein the buffer layer (20) has a thickness of between 10 and 200 nm. 20
[0019]
19. A method of manufacturing a semiconductor structure based on element III nitrides, comprising the steps of: - providing a support according to any one of claims 13 to 18, - growing (300) a semiconductor structure based on element III nitrides (40) on the crystalline layer (30). 25
[0020]
20. The method according to the preceding claim, wherein the growth step (300) comprises a step of deposition of a gallium nitride GaN layer on the crystalline layer (30). 30
[0021]
21. The method according to one of claims 19 or 20, wherein the growth step (300) consists of an organometallic vapor phase epitaxial deposition. 3031834
[0022]
22. Semiconductor structure based on element nitrides III, characterized in that said structure comprises: - a support according to any one of claims 13 to 18, - a semiconductor material based on element nitrides III on the crystalline layer (30).
[0023]
23. Structure according to the preceding claim, wherein the semiconductor material based on element III nitrides on the crystalline layer (30) comprises a layer of gallium nitride. 10
[0024]
24. Structure according to the preceding claim, wherein the gallium nitride GaN has a through dislocation density less than or equal to 5.108 CM-2. 15
[0025]
25. Structure according to the preceding claim, wherein the semiconductor material based on element III nitrides on the crystalline layer (30) comprises an aluminum-based layer.
[0026]
26. Electroluminescent diode based on nitrides of elements III, characterized in that it comprises - a semiconductor structure according to one of claims 22 to 25, - a first contact layer based on gallium nitride disposed on the first element III nitride semiconductor layer; - a second gallium nitride contact layer disposed on the first gallium nitride contact layer; a multiple quantum well structure disposed between the first gallium nitride contact layer and the second gallium nitride contact layer.
类似技术:
公开号 | 公开日 | 专利标题
US8803189B2|2014-08-12|III-V compound semiconductor epitaxy using lateral overgrowth
FR2860248A1|2005-04-01|PROCESS FOR PRODUCING AUTOMATED SUBSTRATES OF ELEMENT III NITRIDES BY HETERO-EPITAXIA ON A SACRIFICIAL LAYER
WO2014064395A1|2014-05-01|Optoelectronic device and method for manufacturing same
EP2997598A1|2016-03-23|Optoelectronic device and method for manufacturing same
EP3248213A1|2017-11-29|Production of a semiconductor support based on group iii nitrides
FR2888039A1|2007-01-05|Fabrication of nitride-based compound layer used in vertical structure nitride-based semiconductor light-emitting device involves laterally growing nitride-based compound from buffer layer to mask layer on gallium nitride substrate
WO2014184487A1|2014-11-20|Optoelectronic device and method for manufacturing same
EP3248212B1|2021-08-18|Method for producing a passivated semiconductor structure based on group iii nitrides, and one such structure
FR2908925A1|2008-05-23|III-IV type component i.e. gallium nitride, integrating method for e.g. LED, involves forming intermediate layer on host zones, suppressing masking and polycrystalline layers, and integrating structures on non host zones
FR3003397A1|2014-09-19|Semiconductor structures with active regions including INGAN
FR3032064A1|2016-07-29|OPTOELECTRONIC DEVICE AND METHOD FOR MANUFACTURING THE SAME
EP3241246A1|2017-11-08|Process for fabricating semiconductor nanowires or microwires having insulated roots
US10354865B2|2019-07-16|Method for producing a nitride compound semiconductor device
EP3384521A1|2018-10-10|Method for obtaining a semi-polar nitride layer on a crystalline substrate
EP3053201B1|2019-10-30|Optoelectronic device based on light-emitting diodes
WO2015177220A1|2015-11-26|Method for manufacturing a semiconductor material including a semi-polar iii-nitride layer
WO2016000990A1|2016-01-07|Optoelectronic device having semiconductor elements and method for manufacturing same
EP3809450A1|2021-04-21|Method for hetero-integration of a semiconductor material of interest in a silicon substrate
WO2014114730A1|2014-07-31|Method for the production of a layer comprising group-iii-element nitride by means of spontaneous delamination
EP3227906B1|2021-11-24|Electronic device with a wire element extending from an electroconductive layer comprising zirconium carbide or hafnium carbide
FR3029942A1|2016-06-17|METHOD FOR MANUFACTURING NITRIDE PLATELETS OF ELEMENT 13 WITH NON-NULL TRUNCATURE ANGLE
FR3048002A1|2017-08-25|PROCESS FOR OBTAINING ON A CRYSTALLINE SUBSTRATE A SEMICOPOLY NITRIDE LAYER
FR3026564A1|2016-04-01|OPTOELECTRONIC DEVICE WITH THREE DIMENSIONAL SEMICONDUCTOR ELEMENTS
同族专利:
公开号 | 公开日
CN107251189B|2020-11-20|
WO2016116715A1|2016-07-28|
US20180019120A1|2018-01-18|
FR3031834B1|2018-10-05|
KR20170102022A|2017-09-06|
CN107251189A|2017-10-13|
US10522346B2|2019-12-31|
EP3248213A1|2017-11-29|
JP2018509755A|2018-04-05|
JP6666353B2|2020-03-13|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
US20040137732A1|2000-07-07|2004-07-15|Eric Frayssinet|Process for producing an epitaxial layer of gallium nitride|
US20020069817A1|2000-07-21|2002-06-13|Mishra Umesh Kumar|Method to reduce the dislocation density in group III-nitride films|
US20120091467A1|2006-05-09|2012-04-19|The Regents Of The University Of California|IN-SITU DEFECT REDUCTION TECHNIQUES FOR NONPOLAR AND SEMIPOLAR N|
US20130178050A1|2010-02-04|2013-07-11|Yong-jin Kim|Method for manufacturing gallium nitride wafer|WO2018091502A1|2016-11-18|2018-05-24|Centre National De La Recherche Scientifique|Semiconductor heterostructures with wurtzite-type structure on zno substrate|AU2430401A|1999-12-13|2001-06-18|North Carolina State University|Methods of fabricating gallium nitride layers on textured silicon substrates, and gallium nitride semiconductor structures fabricated thereby|
DE10151092B4|2001-10-13|2012-10-04|Azzurro Semiconductors Ag|Method for producing planar and crack-free Group III nitride-based light emitting structures on silicon substrate|
JP4963816B2|2005-04-21|2012-06-27|シャープ株式会社|Nitride semiconductor device manufacturing method and light emitting device|
DE102007057241A1|2007-11-28|2009-06-04|Osram Opto Semiconductors Gmbh|Method for producing a stack of layers on a crystalline substrate, which is free from nitride compound semiconductor by using metal organic gas-phase deposition, comprises forming a nitride-containing buffer layer on the substrate|
JP5355158B2|2009-03-13|2013-11-27|株式会社東芝|Semiconductor substrate and semiconductor element|
JP5767015B2|2011-05-10|2015-08-19|出光興産株式会社|thin film transistor|
JP2014009156A|2012-06-29|2014-01-20|Samsung Corning Precision Materials Co Ltd|Method for producing gallium nitride substrate and gallium nitride substrate produced thereby|US10297445B2|2016-06-14|2019-05-21|QROMIS, Inc.|Engineered substrate structure for power and RF applications|
US10510582B2|2016-06-14|2019-12-17|QROMIS, Inc.|Engineered substrate structure|
JP2020145331A|2019-03-07|2020-09-10|株式会社東芝|Semiconductor device|
法律状态:
2015-12-22| PLFP| Fee payment|Year of fee payment: 2 |
2016-07-12| PLFP| Fee payment|Year of fee payment: 3 |
2016-07-22| PLSC| Publication of the preliminary search report|Effective date: 20160722 |
2016-12-21| PLFP| Fee payment|Year of fee payment: 3 |
2018-01-31| PLFP| Fee payment|Year of fee payment: 4 |
2020-01-30| PLFP| Fee payment|Year of fee payment: 6 |
2021-01-28| PLFP| Fee payment|Year of fee payment: 7 |
2022-01-31| PLFP| Fee payment|Year of fee payment: 8 |
优先权:
申请号 | 申请日 | 专利标题
FR1550462A|FR3031834B1|2015-01-21|2015-01-21|FABRICATION OF A SEMICONDUCTOR SUPPORT BASED ON ELEMENT III NITRIDE|
FR1550462|2015-01-21|FR1550462A| FR3031834B1|2015-01-21|2015-01-21|FABRICATION OF A SEMICONDUCTOR SUPPORT BASED ON ELEMENT III NITRIDE|
PCT/FR2016/050126| WO2016116715A1|2015-01-21|2016-01-21|Production of a semiconductor support based on group iii nitrides|
KR1020177023094A| KR20170102022A|2015-01-21|2016-01-21|Fabrication of Group III nitride-based semiconductor supports|
US15/545,288| US10522346B2|2015-01-21|2016-01-21|Production of a semiconductor support based on group III nitrides|
JP2017538731A| JP6666353B2|2015-01-21|2016-01-21|Production of semiconductor supports based on group III nitrides|
CN201680009848.8A| CN107251189B|2015-01-21|2016-01-21|Production of semiconductor carriers based on nitrides of group III elements|
EP16703350.5A| EP3248213A1|2015-01-21|2016-01-21|Production of a semiconductor support based on group iii nitrides|
[返回顶部]