专利摘要:
A surface treatment method of a steel part to give it a high resistance to wear and corrosion comprises a nitriding or nitrocarburizing step adapted to form a combination layer of at least 8 microns thick formed of iron nitrides of ε and / or γ 'phases, an oxidation step suitable for generating a layer of oxides with a thickness of between 0.1 and 3 microns and a step of impregnation by dipping in a impregnation bath during at least 5 minutes at room temperature, this bath consisting of at least 70% by weight, to within 1%, of a solvent formed of a mixture of hydrocarbons formed from a section of alkanes of C9 to C17 from 10% to 30% by weight, to within 1%, of at least one paraffin oil composed of a section of C16 to C32 alkanes and at least one synthetic phenolic additive additive at a concentration of between 0.01% and 3% by weight, to the nearest 0.1%.
公开号:FR3030578A1
申请号:FR1463252
申请日:2014-12-23
公开日:2016-06-24
发明作者:Pierre-Louis Magdinier;Marie-Noelle Desbouche-Janny
申请人:HEF SAS;
IPC主号:
专利说明:

[0001] The invention relates to a method for surface treatment of a ferrous metal part, in practice made of alloy steel or not, having a good resistance to corrosion due to an impregnation treatment. More generally, the invention applies to any type of mechanical parts intended to ensure in service a mechanical function and having a high hardness, a long resistance to corrosion and wear. This is for example the case of many parts used in the field of automotive or aeronautics. To improve the corrosion resistance of mechanical steel parts, various treatments have been proposed, which include a nitriding or nitrocarburizing step (in molten salt baths or in a gaseous medium), sometimes followed by an oxidation step. and / or the deposition of a topcoat. It is recalled that nitriding and nitrocarburizing are thermochemical treatments of nitrogen (respectively nitrogen and carbon) by combination-diffusion: it forms on the surface a combination layer formed of nitrides of iron (there exists several possible phases), under which nitrogen is present by diffusion. Thus, the document EP-0 053 521 proposed, mainly for piston pins whose corrosion resistance and / or coefficient of friction was to be improved, a nitrocarburizing treatment adapted to form an Epsilon phase layer and a finishing treatment consisting in covering the Epsilon layer with a topcoat made of a resin (the document mentions a very wide range, including acrylic resins, alkyds, maleic esters, epoxides, formaldehyde, phenolics, butyral-polyvinyl, polyvinyl chlorides, polyamides, polyimides, polyurethanes, silicones, polyvinyl ethers and urea-formaldehyde, advantageously loaded with additives chosen from zinc phosphates and chromates (to improve corrosion resistance), and / or silicone, waxes, poly-tetrafluoroethylenes, molybdenum di-sulfite, graphite or zinc stearate (for reduce the coefficient of friction). There is no precise result; it is simply mentioned that a good example is a system of acrylic / epoxy / amino resins, containing chromate or zinc stearate or a wax. Document EP-0 122 762 describes a method of manufacturing corrosion-resistant steel parts, comprising nitriding steps (in the Epsilon phase, as above), then gas-phase oxidation, and then application of waxy material (Castrol V425) containing aliphatic hydrocarbons and Group 2a metal soaps, preferably calcium and / or barium soaps. The resistance to salt spray corrosion was of the order of 250 hours.
[0002] The Applicant has itself proposed treatment processes to obtain even better outfits to corrosion. In EP-0 497 663, it has proposed a method of subjecting ferrous metal parts to nitriding, typically to a molten salt bath consisting of cyanates and sodium, potassium and lithium, followed by bath oxidation. of molten salts or in an oxidizing ionizing atmosphere, so as to obtain a nitrided layer comprising a deep and compact underlayer and a well-controlled surface layer of porosity and finally to deposit a polymer with a thickness of between 3 and 20 pm, fluoroethylene-propylene (FEP), or even polytetrafluoroethylene (PTFE), or even polymers or copolymers of fluorinated or silicone polyurethanes, or polyamide-polyimides. With this method, tests have shown that the resistance to corrosion was improved by obtaining exposure to salt spray (BS) ranging from 500 to about 1000 hours without showing a manifestation of corrosion.
[0003] Then, by the document EP-0 524 037, it was proposed a treatment process according to which the parts are nitrided preferably in molten salt baths based on cyanate ions and then oxidized and finally impregnated with a hydrophobic wax. Nitriding followed by oxidation leads to the formation of a layer consisting of a compact deep sub-layer and a surface layer whose porosity is well controlled. The impregnating wax is an organic compound with a high molecular weight of between 500 and 10,000 and a surface tension in the liquid state of between 10 and 73 mN / m. The contact angle between the solid phase and the surface layer and the wax in the liquid state is between 0 and 75 degrees. More specifically, the wax is chosen from natural waxes, synthetic waxes polyethylenes, polypropylenes, polyesters, fluorinated or modified petroleum residues. This solution simultaneously improves the corrosion resistance and friction properties of ferrous metal parts. The parts thus treated have a good resistance to corrosion in standardized salt spray combined with good friction properties. EP-0 560 641 discloses a process for the phosphating of steel parts to improve the corrosion and wear resistance, making it possible to obtain specific surface characteristics resulting from a phosphating treatment preceded by a nitriding in a bath of molten salts containing sulfur species, a nitriding operation in a molten salt bath followed by a conventional sulfurization treatment, or a metal deposition followed by a conventional sulfurization operation. The corrosion resistance values of the parts thus treated, after exposure to salt spray, are of the order of 900 to 1200 hours. EP-1 180 552 relates to a surface treatment process for mechanical parts subjected to both wear and corrosion having a roughness conducive to good lubrication and according to which nitriding is carried out by immersion between 500 ° C and 700 ° C parts in a bath of molten salt nitriding containing alkaline cyanates and carbonates in precise ranges but free of sulfur species, then an oxidation is carried out in an aqueous oxidizing solution below 200 ° C. The document WO2012 / 146839 referred to a nitriding treatment leading to an appropriate roughness without the need for finishing treatment; he has described a bath of molten salts for the nitriding of mechanical steel parts having specific contents of alkali metal chloride, alkali metal carbonate, alkali metal cyanate and cyanide ions. The corrosion resistance measured in salt spray was between 240 and 650 hours.
[0004] It should be noted that the fact of adding a finishing treatment (deposition of a varnish or a wax, or phosphating treatment) to a nitriding or nitrocarburizing treatment and then oxidation of mechanical parts made of ferrous material makes it possible to often to improve the corrosion resistance, but usually involving a surcharge complicating obtaining, at the end of treatment, the desired dimensional dimensions. In the alternative, it has been found that certain finishing treatments result in the fact that the surface of the parts thus treated tends to transfer a little oil to the surfaces with which it can come into contact and tends to pick up the dust. the surrounding environment; this is hardly compatible with a complementary step such as overmolding. The object of the invention is to remedy these disadvantages in a simple, safe, effective and rational manner, while achieving very high levels of resistance to corrosion and to wear, better than with baths. current impregnation.
[0005] To solve such a problem, it has been designed and developed a method of surface treatment of a mechanical part made of steel to give it a high resistance to wear and corrosion comprising: a nitriding or nitrocarburizing step adapted to form a combination layer of at least 8 micrometers thick formed of phase E iron nitrides and / or y ', - an oxidation step adapted to generate a layer of oxides with a thickness of between 0.1 micrometer and 3 micrometers and - a step of impregnation by soaking in an impregnation bath for at least 5 minutes, this bath being formed of at least 70% by weight, to within 1%, of a solvent formed of a mixture of hydrocarbons formed from a C9 to C17 alkane fraction, from 10% to 30% by weight, to within 1%, of at least one paraffin oil composed of a C16 alkane section at C32 and at least one synthetic phenolic additive additive at a concentration of ise between 0.01% and 3% by weight, to 0.1%, at room temperature. It has been found that, provided that nitriding or nitrocarburizing and oxidation have been carried out sufficiently efficiently to form the layers defined above, the impregnation in a bath according to the invention leads to a substantial improvement in the corrosion resistance compared to a conventional bath, based on oils, acids and ethanol. In addition, it has been found that, after the impregnation treatment, the parts are dry to the touch (this is understood to mean the absence of oil transfer on an opposing surface), hence the absence of a tendency to capture surrounding dust and the ability to undergo post-treatment such as overmolding. Thus one can recognize a part according to the invention, obtained by the method of the invention, namely a steel part having a high resistance to wear and corrosion, comprising a combination layer at least 8 microns, a layer of oxides with a thickness between 0.1 and 3 microns and an impregnation layer which is dry to the touch.
[0006] The notion of ambient temperature does not mean a precise temperature but the fact that the treatment is done without control of the temperature (it is thus neither necessary to heat the bath nor to cool it), and that it can be done the temperature induced by the environment, although it varies in proportions that can be significant during the year, for example between 15 ° C and 50 ° C. Preferably, the nitriding / nitrocarburizing step is conducted so that the thickness of the resulting combination layer is at least 10 microns. Advantageously, the synthetic phenolic additive is a compound of formula C15H240. Also advantageously, the impregnation bath 10 further comprises at least one additive selected from the group consisting of calcium or sodium sulfonate, phosphites, diphenylamines, zinc dithiophosphate, nitrites, phosphoramides. The content of such additives is advantageously at most equal to 5%. More particularly, the bath is preferably formed of 90% +/- 0.5% by weight of solvent, 10% +/- 0.5% by weight of paraffin oils and between 0.01% and not more than 1% +/- 0.1% of synthetic phenolic additive of formula C15H240. Advantageously, the impregnation is carried out by soaking for a period of about 15 minutes. This dipping step is advantageously followed by a natural drying operation or accelerated by steaming. According to a first advantageous option, the nitriding / nitrocarburizing step is carried out in a bath of molten salts containing from 14% to 44% by weight of alkaline cyanates at a temperature of 550 ° C. to 650 ° C. for at least 45 minutes. ; preferably, this nitriding / nitrocarburizing bath contains from 14% to 18% by weight of alkaline cyanates. Advantageously, this treatment is carried out at a temperature of 590 ° C for 90 minutes to 100 minutes; according to a variant, also advantageous, the nitriding / nitrocarburizing treatment in molten salt baths is carried out at a temperature of 630 ° C for about 45 minutes to 50 minutes. According to a second advantageous option, the nitriding / nitrocarburizing step is carried out in a gaseous medium between 500 ° C. and 600 ° C. containing ammonia. According to a third advantageous option, the nitriding / nitrocarburizing step is carried out in an ionic medium (plasma) in a medium comprising at least nitrogen and hydrogen under reduced pressure. Advantageously, the oxidation step is carried out in a bath of molten salts containing carbonates, nitrates and alkali hydroxides. According to a particularly interesting option, the bath of molten oxidation salts contains alkaline nitrates, alkaline carbonates and alkali hydroxides. In this case, it is advantageous that the oxidation step is carried out at a temperature of 430 ° C to 470 ° C for 15 to 20 minutes. According to another interesting option, the oxidation is carried out in an aqueous bath containing alkali hydroxides, alkaline nitrates and alkaline nitrites. In this case, it is advantageous that the oxidation step is carried out at a temperature of 110 ° C to 130 ° C for 15 to 20 minutes. Alternatively, the oxidation step is carried out in a gaseous medium consisting predominantly of water vapor at a temperature of 450 ° C to 550 ° C for 30 to 120 minutes. These various preferences are apparent from various tests that have been carried out, by way of nonlimiting illustrative example. More specifically, these tests were carried out by combining several types of nitriding or nitrocarburizing treatments, known per se, several types of oxidation treatment, known per se, and several types of impregnation. These tests were performed on ferrous metal parts with smooth areas and sharp edges. More particularly, tests have been carried out on annealed and rectified XC45 steel splined shafts having a smooth bearing and a threaded bearing. In total, five nitriding or nitrocarburizing treatments were tested. Three of these treatments are molten salt bath treatments, NITRU1 to NITRU3, which correspond to examples of nitrocarburizing in accordance with the nitrocarburizing treatment taught by the document EP-1 180 552 with: the treatment NITRU1 located in a low temperature range preferred and the preferred average treatment time (from 45 minutes to 50 minutes), * the NITRU2 treatment located in this same low temperature range preferred but with the maximum treatment time (outside the preferred zone, ie from 90 minutes to 100 minutes) and * the NITRU3 treatment at the preferred high temperature range with the preferred average treatment time (45 minutes to 50 minutes). The parameters of these treatments are summarized in the table below. Content in Temperature Temperature Time of Layer Thickness CN- in ° A> CNCY in ° A> (in ° C) treatment (in treatment (in (by weight) (in weight) minutes) micrometers) NITRU1 1 to 3 14 to 18 590> = 45 <8 NITRU 2 1 to 3 14 to 18 590> = 90> 8 NITRU3 1 to 3 14 to 18 630> = 45> 8 More generally, it can be noted that NITRU1 treatment leads to a combination layer of thickness less than 8 micrometers, while the treatments NITRU2 and NITRU3 lead to a layer whose thickness exceeds this threshold, and is preferably even at least 10 micrometers. It seems pointless, in practice, to try to exceed 25 micrometers, so that an effective range for the thickness of the layer seems to be 10 to 25 micrometers. In general, these three treatments correspond to a treatment in a bath of molten salts containing from 14% to 44% by weight of alkaline cyanates (preferably from 14% to 18%) at a temperature of 550 ° C. to 650 ° C. (preferably from 590 ° C to 630 ° C) for at least 45 minutes (it does not seem useful to exceed 120 minutes, or even 90 minutes). Another of these treatments is a conventional gaseous treatment, NITRU4 (aiming a combination layer thickness of at least 8 pm and advantageously between 10 and 2511m), and another of these treatments is a conventional treatment in medium ionic (plasma), NITRU5 (aiming a combination layer thickness of at least 8 pm and advantageously between 10 and 25 pm). More specifically, the NITRU4 treatment in gaseous medium was carried out in an oven between about 500 and 600 ° C under a controlled atmosphere comprising ammonia. The treatment time has been established to ensure a combination layer thickness of at least 8 microns, preferably greater than 10 microns. As for the NITRU5 treatment, it was carried out in an ionic medium (plasma) in a mixture comprising at least nitrogen and hydrogen, under reduced pressure (that is to say at a pressure below atmospheric pressure). typically less than 0.1 atmosphere). The treatment time has also been established to ensure a combination layer thickness of at least 8 microns, preferably at least 10 microns.
[0007] In the above, the indicated treatment layer thickness does not take into account the diffusion layer (for nitrogen as well as for carbon). According to these various nitriding / nitrocarburizing treatments, various combination layers have been obtained: either e-phase nitrides (Fe 2 -3 N) or nitrides in the e and Y 'phases (Fe 2 -3 N + Fe 4 N) with the salt baths NITRU 1 to NITRU 3 and nitrides in phases e and Y '(Fe 2 -3N + Fe 4 N) with the gas phase treatment NITRU 4, nitrides in the e and Y' phases (Fe 2 3 N + Fe 4 N) with the NITRU 5 plasma phase treatment. Only NITRU2 to NITRU5 treatments resulted in combination layer thicknesses of at least 8 microns, preferably between 10 and 25 microns.
[0008] For each of the 5 nitriding treatments NITRU1 to NITRU5, three types of oxidation treatments were implemented: 1) Oxidation "type 1" (or 0x1), that is to say in an ionic liquid medium containing NaNO 3 (between 35 and 40% by weight), carbonates (Li, K, Na) (between 15 and 20% by weight), NaOH (between 40 and 45% by weight) - temperature of 450 ° C - treatment time of 15 minutes. 2) "Type 2" oxidation (or 0x2, ie in an aqueous medium containing KOH (between 80% and 85% by weight, NaNO3 (between 10% and 15% by weight and NaNO2 (between 1 and 6% by weight - temperature of 120 ° C - treatment time of 15 minutes 3) Oxidation "type 3" (or 0x3) in a gaseous medium (treatment with water vapor) - temperature of 500 ° C - time The oxidations 0x1 and 0x2 substantially correspond, respectively, to the oxidation in a salt bath and to the aqueous oxidation of the aforementioned document EP1180552, whereas the parameters of nitrocarburizing treatments (NITRU5) and of oxidation treatments are as follows: 0x3, in an ionized medium, correspond substantially to Example 9 of EP0497663, the oxidations being carried out so as to obtain oxidation layers having a thickness of between 0.1 and 3 micrometers. oxidation, two types of impregnation have been realized: 1) a new impregnation called "impregnation 1" (or Imp1) in a bath containing mainly a solvent (90% +/- 0.5% by weight) formed of a mixture of hydrocarbons composed of a C9 to C17 alkane cut, 10% +/- 0.5% by weight a paraffin oil composed of a C16 to C32 alkane cut and between 0.1% and 1% + 10.1% of a synthetic phenolic additive of formula C15H240. This impregnation was performed by dipping for about 15 minutes of immersion, followed by natural drying or accelerated by steaming. 2) A conventional impregnation called "impregnation 2" (or Imp2), in a bath containing mainly oils (between 60 and 85% by weight), acids (between 6 and 15% by weight) and ethanol (between 1 and 5% by weight). This impregnation was carried out by dipping for about 15 minutes immersion, followed by natural drying or accelerated by steaming. By combining the types of oxidation and the types of impregnation, 8 treatments, denoted 1 to 8, were defined in accordance with the following table (denoted an absence of oxidation by "0x0").
[0009] Type of oxidation Type of impregnation Treatment 1 0x1 Imp2 Treatment 2 0x1 Imp1 Treatment 3 0x2 Imp2 Treatment 4 0x2 Imp1 Treatment 5 0x3 Imp2 Treatment 6 0x3 Imp1 Treatment 7 Oxidation-free (0x0) Imp2 Treatment 8 Oxidation-free (0x0) Imp1 Samples were prepared by combining these treatments 1 to 8 with the aforementioned nitriding / nitrocarburizing treatments. Corrosion resistance tests were performed according to ISO 9227 (2006) in salt spray. The results are summarized in the table below. For each test, a minimum of 10 pieces has been tested. The time (indicated in hours) corresponds to a total absence of trace of corrosion on 100% of the parts.
[0010] It appeared that the impregnation treatment 1 did not induce dimensional variation. In addition, the surface of the pieces was dry to the touch; this implies that, on the one hand, the surface of these parts does not have a tendency to capture the dust and that, on the other hand, these parts are compatible with a post-treatment such as an overmoulding.15 Without NITRU 1 NITRU 2 NITRU 3 NITRU 4 NITRU 5 Nitriding Treatment 1 96h 360h 912h 792h 384h 72h Ox1 + Imp2 Treatment 2 96h 960h 1368h 1368h 1008h 576h Ox1 + Imp1 Treatment 3 96h 312h 576h 792h 504h 72h Ox2 + Imp2 Treatment 4 96h 360h 1056h 1056h 720h 360h Ox2 + Imp1 Treatment 5 96h 192h 456h 552h 312h 24h Ox3 + Imp2 Treatment 6 96h 264h 888h 792h 552h 72h Ox3 + Imp1 Treatment 7 96h 96h 456h 384h 48h 48h Ox0 + Imp2 Treatment 8 96h 120h 504h 624h 360h 336h Ox0 + Imp1 All in all first of this table that the new treatment of impregnation (impregnation 1 - even treatments) brings a significant improvement compared to the case of a traditional impregnation (impregnation 2 - odd treatments). It can be noted that the oxidation-impregnation treatment is of little importance when there is no nitriding / nitrocarburization (the corrosion resistance remains at 96h, in the first column). As for the NITRU5 treatment, it tends to show that the impregnation treatment 2 (conventional) results in a lower corrosion resistance to the case without any nitriding.
[0011] The interest of type 1 impregnation is particularly visible in the case of NITRU5 nitrocarburizing since, with the case of oxidation 3 (in a gaseous medium - treatments 5 and 6), the improvement is of the order of a tripling of the resistance to corrosion (increase of about fifty hours) compared to the case of a conventional impregnation; it is nevertheless the case where the oxidation has a particularly negative effect. In all other cases NITRU5, the increase in corrosion resistance is at least of the order of 200 hours. Thus, in the case of NITRU5 combined with oxidation in an aqueous medium (oxidation 2 - treatments 3 and 4) or in the absence of oxidation (treatments 7 and 8), the new impregnation results in an increase in resistance to corrosion of the order of 300 hours; in the case of NITRU5 combined with oxidation in an ionic liquid medium (oxidation 1 - treatments 1 and 2), the increase is even of the order of 500 hours.
[0012] With regard to the NITRU1 treatment, it can be noted that the beneficial effect of the new impregnation exists but is moderate, including in percentage, compared with the conventional impregnation (treatments 3 to 8, even if the suits at the corrosion, in absolute value, are better than with NITRU5). However, we can note a very important increase, of 600 hours, in the case of an oxidation in ionic medium (treatments 1 and 2), with a resistance to the corrosion approaching threshold of 1000 hours. It can be inferred that the condition of a combination layer of at least 8 micrometers thick can be lowered in the case of type 1 oxidation.
[0013] If we now consider the NITRU4 treatment, it leads to the same comment as the NITRU5 treatment in the absence of oxidation (treatments 7 and 8). On the other hand, there is an increase of at least 200 hours of corrosion resistance in the case of oxidation type 2 (in aqueous medium - treatments 3 and 4) and type 3 (in gaseous medium - treatments 5 and 6) . However, a remarkable increase is observed in the case of a type 1 oxidation (oxidation in high temperature ionic medium - treatments 1 and 2), since the corrosion resistance is improved by nearly 600 hours by exceeding the threshold of 1000 hours. If one now considers nitriding / nitrocarburizing treatments in molten salt baths in which care has been taken to obtain a combination layer at least 8 micrometers thick (or even 10 micrometers), it can be seen that New impregnation leads to particularly high levels of corrosion resistance. In the case of an absence of oxidation, the new impregnation brings an improvement, especially significant in the case of NITRU3.
[0014] In the presence of oxidation, the improvement in corrosion resistance is, for oxidation of type 2 and 3 (treatments 3 to 6) of at least 250 hours for the treatment NITRU3 and even 450 hours for the treatment NITRU2. With type 2 oxidation (treatments 3 and 4), corrosion resistance exceeding the threshold of 1000 hours is obtained.
[0015] With the oxidation of type 1 (treatments 1 and 2), the increase brought by the new impregnation is surprisingly high, since it is 456 hours for NITRU2 and even 576h for NITRU3 to reach a particularly high threshold, of the order of 1370h. Thus, it appears that: the new impregnation brings about an improvement in the resistance to corrosion compared to a conventional impregnation, whatever the nitriding / nitrocarburizing and oxidation treatments, this improvement is particularly notable and leads to particularly high corrosion resistance values for salt bath nitrocarburizing treatments resulting in a combination layer of at least 8 microns (NITRU2 and NITRU3), preferably between 10 and 25 micrometers, - This improvement is particularly noticeable and leads to particularly high corrosion resistance values for nitrocarburations in salt baths (NITRU1 to NITRU3) or in the gas phase (NITRU4) in the case of molten salt bath oxidation (type 1), - This improvement leads to particularly high levels of corrosion resistance by combining nitrocarburts in salt baths leading to a layer at least 8 micrometers thick (NITRU2 and NITRU3) and type 1 or 2 oxidation, especially in the case of salt bath oxidation (type 1). The above results were measured on smooth areas of the samples. Measurements on areas with asperities (threaded zones in this case) have also shown that the best results are obtained with the liquid oxidation treatments 1 and 2, combined with a type 1 impregnation and nitrocarburizing in salt baths leading to combination layers of at least 8 micrometers, NITRU2 and NITRU3. While the new impregnation results in excellent results, equivalent for NITRU2 and NITRU3, with the oxidations in liquid medium, on smooth surfaces, it seems that, on the non-smooth zones, the new impregnation gives very good results for these two same types of nitrocarburation, a little better with NITRU3 than with NITRU2. In summary, the above results show that the impregnating bath 1 has a surprising synergistic effect with nitriding / nitrocarburizing treatments NITRU2 and NITRU3 provided that nitriding / nitrocarburizing is followed by oxidation of type 1 or 2 , an optimum appearing to be obtained when the oxidation treatment is of type 1.
[0016] The magnitude of the corrosion resistance increases noted for the combination of impregnation bath 1 with nitriding / nitrocarburizing treatments in molten salt baths resulting in combination layers of more than 8 micrometers thick (NITRU2 and NITRU3 ) and the oxidation treatment 1 molten salt bath reflects the existence of a surprising synergy between these three types of treatment that remains misunderstood. The particular composition of the impregnation bath considered in the tests is part of a more general composition, namely a bath consisting of at least 70% by weight, to within 1%, of a solvent formed of a mixture of hydrocarbons. formed from a cut of C9 to C17 alkanes, from 10% to 30% by weight, to within 1%, of at least one paraffin oil composed of a section of C16 to C32 alkanes and from minus a synthetic phenolic additive additive at a concentration of between 0.01% and 3% by weight, at room temperature. The solvent content is preferably between 80% and 90% by weight; likewise, the content of paraffin oil is preferably between 10% and 20% by weight. The alkane section of the solvent is preferably C9 to C14.
[0017] The above results were obtained on the basis of XC45 steel samples, but it is within the abilities of those skilled in the art to adapt the processing parameters according to the material used, and thus follow the aforementioned teaching. 30
权利要求:
Claims (18)
[0001]
REVENDICATIONS1. A method of surface treatment of a steel part to impart a high wear and corrosion resistance comprising a nitriding or nitrocarburizing step adapted to form a combination layer at least 8 micrometers thick formed of phase E iron nitrides and / or y ', * an oxidation step adapted to generate a layer of oxides with a thickness of between 0.1 and 3 microns and a step of impregnation by dipping in a bath 10 d impregnation for at least 5 minutes, this bath consisting of at least 70% by weight, to within 1%, of a solvent formed of a mixture of hydrocarbons formed from a section of C9 to C17 alkanes from 10% to 30% by weight, to within 1%, of at least one paraffin oil composed of a C16 to C32 alkane slice and at least one synthetic phenolic additive additive of one to one concentration between 0.01% and 3% by weight, to the nearest 0.1%, at room temperature.
[0002]
2. The method of claim 1 wherein the synthetic phenolic additive is a compound of formula C15H240.
[0003]
3. A process according to claim 2, wherein the impregnating bath is formed of 90% +/- 0.5% by weight of solvent, 10% +/- 0.5% by weight of paraffin oils and less than 1% +/- 0.1% of synthetic phenolic additive of formula C15H240.
[0004]
4. Process according to any one of claims 1 to 3, wherein the impregnating bath further comprises at least one additive selected from the group consisting of calcium or sodium sulphonate, phosphites, diphenylamines, dithiophosphate. zinc, nitrites, phosphoramides.
[0005]
5. A process according to any one of claims 1 to 4, wherein the soaking operation is followed by a natural drying operation or accelerated by steaming.
[0006]
6. Process according to any one of claims 1 to 5, in which the nitriding or nitrocarburizing step is carried out in a bath of molten salts containing from 14% to 44% by weight of alkaline cyanates at a temperature of 550 ° C. at 650 ° C for at least 45 minutes.
[0007]
The process according to claim 6, wherein the nitriding / nitrocarburizing bath contains from 14% to 18% by weight of alkaline cyanates.
[0008]
The process according to claim 6 or claim 7, wherein the nitriding / nitrocarburizing treatment is carried out at a temperature of 590 ° C for 90 minutes to 100 minutes.
[0009]
9. A process according to claim 6 or claim 7, wherein the nitriding / nitrocarburizing treatment is carried out at a temperature of 630 ° C for about 45 minutes to 50 minutes.
[0010]
The process according to any one of claims 1 to 5, wherein the nitrocarburizing step is carried out in a gaseous medium between 500 ° C and 600 ° C containing ammonia. 20
[0011]
11. A method according to any one of claims 1 to 5, wherein the nitriding or nitrocarburizing step is carried out in an ionic medium forming a plasma, comprising at least nitrogen and hydrogen under reduced pressure.
[0012]
12. A process according to any one of claims 1 to 11, wherein the nitriding or nitrocarburizing step is carried out so as to form a combination layer of thickness at least equal to 10 micrometers.
[0013]
13. A process according to any one of claims 1 to 12, wherein the oxidation step is carried out in a bath of molten salts which contains alkali nitrates, alkali carbonates and alkali hydroxides.
[0014]
The process according to claim 13, wherein the oxidation step is carried out at a temperature of 430 ° C to 470 ° C for 15 to 20 minutes.
[0015]
15. Process according to any one of claims 1 to 12, the oxidation step of which is carried out in an aqueous bath which contains alkali hydroxides, alkaline nitrates and alkaline nitrites. 10
[0016]
The process according to claim 15, wherein the oxidation step is carried out at a temperature of 110 ° C to 130 ° C for 15 to 20 minutes.
[0017]
17. A process according to any one of claims 1 to 12, wherein the oxidation step is carried out in a gaseous medium consisting predominantly of water vapor, at a temperature of 450 ° C to 550 ° C for 30 to 120 minutes.
[0018]
18. A steel piece having a high wear and corrosion resistance obtained by the process of any one of claims 1 to 17, having a combination layer of at least 8 micrometers, an oxide layer thickness between 0.1 and 3 micrometers and an impregnation layer which is dry to the touch.
类似技术:
公开号 | 公开日 | 专利标题
CA2968630C|2019-08-27|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating
FR2731232A1|1996-09-06|METHOD OF TREATING FERROUS SURFACES SUBJECTED TO HIGH FRICTIONAL SOLLICITATIONS
EP0524037B1|1995-04-19|Treatment process for iron components to improve simultaneously their corrosion resistance and their friction properties
EP0497663B2|2002-10-09|Method of manufacturing corrosion resistant steel components and keeping their friction properties by nitriding and then oxidizing them
EP2683845B1|2019-06-26|Salt bath for nitriding of steel workpieces and its related production method
WO2013117759A1|2013-08-15|Method for anodizing parts made of an aluminum alloy
EP1180552B1|2011-02-16|Method for surface treatment of mechanical pieces subjected to wear and corrosion
EP1875092B1|2019-10-16|Pair of guiding elements of which one is made of a specific steel leading to improved anti-seizing performances
EP2082014A2|2009-07-29|Watch
EP1801262B1|2008-11-26|Treatment by carboxylation of metal surfaces, use of this process as temporary protection against corrosion and manufacturing process of a shaped sheet coated with a carboxylated conversion coating
WO2021130460A1|2021-07-01|Method for treating a part made of ferrous metal, and part made of ferrous metal
JP6915549B2|2021-08-04|Sliding member and its manufacturing method
JP2017160538A|2017-09-14|Diamond like carbon film, sliding member, processing member, and method for manufacturing diamond like carbon film
同族专利:
公开号 | 公开日
US10774414B2|2020-09-15|
SI3237648T1|2020-09-30|
JP6608450B2|2019-11-20|
AU2015370805A1|2017-08-10|
RU2017126188A|2019-01-24|
EP3237648B1|2020-03-18|
KR20170097736A|2017-08-28|
CA2968630A1|2016-06-30|
JP2018502220A|2018-01-25|
CN107109617A|2017-08-29|
AU2015370805B2|2020-10-15|
TWI683036B|2020-01-21|
RU2017126188A3|2019-06-07|
SG11201704798RA|2017-07-28|
ES2785599T3|2020-10-07|
BR112017011508B1|2021-08-10|
US20170349997A1|2017-12-07|
CA2968630C|2019-08-27|
FR3030578B1|2017-02-10|
TN2017000216A1|2018-10-19|
DK3237648T3|2020-05-11|
WO2016102813A1|2016-06-30|
MX2017008334A|2018-04-24|
TW201631183A|2016-09-01|
PL3237648T3|2020-08-24|
EP3237648A1|2017-11-01|
HUE049293T2|2020-09-28|
PT3237648T|2020-05-27|
ZA201704730B|2018-05-30|
BR112017011508A2|2018-02-27|
CN107109617B|2020-01-14|
RU2696992C2|2019-08-08|
PH12017500936A1|2017-11-20|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
EP0497663A1|1991-01-30|1992-08-05|CENTRE STEPHANOIS DE RECHERCHES MECANIQUES HYDROMECANIQUE ET FROTTEMENT Société dite:|Method of manufacturing corrosion resistant steel components and keeping their friction properties by nitriding and then oxidizing them|
EP0524037A1|1991-07-16|1993-01-20|CENTRE STEPHANOIS DE RECHERCHES MECANIQUES HYDROMECANIQUE ET FROTTEMENT Société dite:|Treatment process for iron components to improve simultaneously their corrosion resistance and their friction properties|
KR100215252B1|1991-07-16|1999-08-16|쥐. 엘 뽈띠|Ferrous metal partswith simultaneously improved corrosion resistance and friction properties|
EP1180552A1|2000-08-14|2002-02-20|CENTRE STEPHANOIS DE RECHERCHES MECANIQUES HYDROMECANIQUE ET FROTTEMENT Société dite:|Method for surface treatment of mechanical pieces subjected to wear and corrosion|FR3105262A1|2019-12-24|2021-06-25|H.E.F.|Method and installation for treating a piece of ferrous metal|JPS55125267A|1979-03-22|1980-09-26|Kawasaki Heavy Ind Ltd|Surface treating method of improving abrasion resistance and corrosion resistance of iron and steel|
JPS57141464A|1980-12-03|1982-09-01|Lucas Industries Ltd|Metal member working method|
BR8107846A|1980-12-03|1982-09-08|Lucas Industries Ltd|STEEL METAL COMPONENT|
EP0074211B1|1981-09-05|1987-11-04|LUCAS INDUSTRIES public limited company|Coated metal substrate and method of coating a metal substrate|
ZA827448B|1981-10-15|1983-08-31|Lucas Ind Plc|Corrosion resistant steel components and method of manufacture thereof|
JPS5977138A|1982-10-26|1984-05-02|Aisin Chem Co Ltd|Friction material for vehicle|
GB8310102D0|1983-04-14|1983-05-18|Lucas Ind Plc|Corrosion resistant steel components|
JPH0257735A|1988-08-19|1990-02-27|Toyoda Gosei Co Ltd|Vibration preventing rubber|
DE4027011C2|1990-08-27|1992-10-29|Degussa Ag, 6000 Frankfurt, De|
FR2688517B1|1992-03-10|1994-06-03|Stephanois Rech|PROCESS FOR THE PHOSPHATION OF STEEL PARTS, TO IMPROVE THEIR CORROSION AND WEAR RESISTANCES.|
JPH083721A|1994-06-13|1996-01-09|Kayaba Ind Co Ltd|Surface treatment of piston rod|
US5714015A|1996-04-22|1998-02-03|Frantz Manufacturing|Ferritic nitrocarburization process for steel balls|
JP2001323939A|2000-05-18|2001-11-22|Nsk Ltd|Rolling bearing|
JP4998654B2|2001-01-31|2012-08-15|日立オートモティブシステムズ株式会社|Method of gas soft nitriding treatment of steel members|
RU2230824C2|2002-04-09|2004-06-20|Общество с ограниченной ответственностью "Борец"|Method of chemicothermal treatment of a material on the base of iron alloy, the material on the base of iron alloy and a component of a block of an immersion centrifugal pump|
RU2230825C2|2002-08-30|2004-06-20|Общество с ограниченной ответственностью "Борец"|Method of chemicothermal treatment of a material on the base of powder alloys of iron and a component of a block of an immersion centrifugal pump|
FR2972459B1|2011-03-11|2013-04-12|H E F|FOUNDED SALT BATHS FOR NITRIDING STEEL MECHANICAL PARTS, AND METHOD FOR IMPLEMENTING THE SAME|CN108359785B|2018-03-19|2019-12-17|盐城工学院|Strengthening and toughening treatment method for W6Mo5Cr4V2 high-speed steel broach|
CN110423977B|2019-09-05|2021-06-18|合肥工业大学|Gas nitriding method for aluminum material by taking chemical iron-immersion plating as pretreatment|
RU2737796C1|2020-03-05|2020-12-03|Федеральное государственное бюджетное образовательное учреждение высшего образования "Ростовский государственный университет путей сообщения" |Compound composition for nitriding parts from alloyed steels|
RU2736289C1|2020-03-05|2020-11-13|Федеральное государственное бюджетное образовательное учреждение высшего образования "Ростовский государственный университет путей сообщения" |Method of nitriding parts from alloyed steels|
CN111423817A|2020-05-28|2020-07-17|眉山市三泰铁路车辆配件有限公司|Special gas QPQ coupling agent for cast iron product and preparation method thereof|
法律状态:
2015-11-06| PLFP| Fee payment|Year of fee payment: 2 |
2016-06-24| PLSC| Search report ready|Effective date: 20160624 |
2016-11-25| PLFP| Fee payment|Year of fee payment: 3 |
2017-11-10| PLFP| Fee payment|Year of fee payment: 4 |
2019-12-04| PLFP| Fee payment|Year of fee payment: 6 |
2020-12-28| PLFP| Fee payment|Year of fee payment: 7 |
优先权:
申请号 | 申请日 | 专利标题
FR1463252A|FR3030578B1|2014-12-23|2014-12-23|PROCESS FOR SUPERFICIAL TREATMENT OF A STEEL PART BY NITRURATION OR NITROCARBURING, OXIDATION THEN IMPREGNATION|FR1463252A| FR3030578B1|2014-12-23|2014-12-23|PROCESS FOR SUPERFICIAL TREATMENT OF A STEEL PART BY NITRURATION OR NITROCARBURING, OXIDATION THEN IMPREGNATION|
JP2017533624A| JP6608450B2|2014-12-23|2015-12-15|Method of surface treatment of steel parts by nitriding or soft nitriding, oxidation and subsequent impregnation|
MX2017008334A| MX2017008334A|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating.|
KR1020177020140A| KR20170097736A|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
RU2017126188A| RU2696992C2|2014-12-23|2015-12-15|Method of surface treatment of steel part by nitration or nitrogen-carbonisation, oxidation, and then with impregnation|
PT158211250T| PT3237648T|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
AU2015370805A| AU2015370805B2|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
SI201531209T| SI3237648T1|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
PCT/FR2015/053511| WO2016102813A1|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
SG11201704798RA| SG11201704798RA|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
PL15821125T| PL3237648T3|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
HUE15821125A| HUE049293T2|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
ES15821125T| ES2785599T3|2014-12-23|2015-12-15|Surface treatment process of a steel part by nitriding or nitrocarburizing, oxidation and then impregnation|
CN201580070179.0A| CN107109617B|2014-12-23|2015-12-15|Method for treating the surface of a steel component by nitriding or carbonitriding, oxidation and subsequent impregnation|
CA2968630A| CA2968630C|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
US15/538,005| US10774414B2|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
DK15821125.0T| DK3237648T3|2014-12-23|2015-12-15|Process for surface treatment of a steel component by nitration or nitrocarburization, oxidation and then impregnation|
BR112017011508-5A| BR112017011508B1|2014-12-23|2015-12-15|SURFACE TREATMENT PROCESS OF A STEEL PART BY NITERING OR NITROCARBONIZATION, OXIDATION FOLLOWED BY IMPREGNATION AND STEEL PART|
EP15821125.0A| EP3237648B1|2014-12-23|2015-12-15|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
TN2017000216A| TN2017000216A1|2014-12-23|2015-12-15|PROCESS FOR THE SUPERFICIAL TREATMENT OF A STEEL PART BY NITRURATION OR NITROCARBURING, OXIDATION THEN IMPREGNATION|
TW104143194A| TWI683036B|2014-12-23|2015-12-22|Method of surface treatment of a steel part by nitriding or nitrocarburizing, oxidation then impregnation|
PH12017500936A| PH12017500936A1|2014-12-23|2017-05-19|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
ZA2017/04730A| ZA201704730B|2014-12-23|2017-07-13|Method for surface treatment of a steel component by nitriding or nitrocarburising, oxidising and then impregnating|
[返回顶部]