专利摘要:
A high strength alkaline borosilicate glass is disclosed. Alkaline borosilicate glass consists of the following components: SiO2 70 - 86% by weight Al2O3 0 - 5% by weight B2O3 9.0 - 25% by weight Na2O 0.5 - 5.0% by weight K2O 0 - 1.0% by weight Li2O 0 - 1.0% by weight, as well as 0 - 5.0% by weight of other components. The proportions of the components are chosen such that the weighted crosslinking index, i.e. the average number n of stress conditions per atom, has a value greater than 2.9, preferably greater than 2.91, particularly advantageously greater than 2.92, and especially greater than 2.93.
公开号:FR3030488A1
申请号:FR1563267
申请日:2015-12-23
公开日:2016-06-24
发明作者:Gerhard Lautenschlager;Jochen Alkemper;Ulf Dahlmann;Ulrich Fotheringham
申请人:Schott AG;
IPC主号:
专利说明:

[0001] The present invention relates to a solid alkaline borosilicate glass, as well as to a process for producing and using the same. Alkaline borosilicate glasses are known per se and are commercially available, for example under the following trade names: Duran, Borofloat 33 or also Pyrex. Duran contains, for example, 80.2% by weight of SiO 2, 13.4% by weight of B 2 O 3, 2.3% by weight of Al 2 O 3, 3.5% by weight of Na 2 O and 0.6% by weight of K 2 O. Alkaline borosilicate glasses are characterized by low temperature sensitivity and dimensional stability up to high temperatures. In addition, when in contact with liquids, glasses of this type have excellent chemical resistance. For this reason, these glasses are used as for a large number of applications in the field of household glass and hotel and restaurant glass. These types of glass are used in particular in laboratories, but also in the construction of industrial installations. Thus, for example, glass pipes of any length are used for sewage gas or for the transfer of aggressive chemicals. Another area of use is the pharmaceutical industry.
[0002] Alkaline borosilicate glasses are also used in the field of electrical engineering for electrical insulation purposes. On the other hand, the use of glass is spreading more and more in the building industry, for example for the realization of facades, for guardrails, roofs, doors as well as for partitions. This presents increased risks in case of fire. Conventional flat glasses are already breaking in a short time under the effect of heat on one side, and large fragments detach and allow the fire to spread in nearby rooms. To avoid this, it has been attempted in the past to prevent the rupture of windows by incorporating a wire mesh, so that when a window breaks, its fragments are retained in the structure by the wire mesh. Fire resistant glazing has already been developed which meets the requirements of fire resistance ratings G and F (DIN 4102 Part 13 (ISO 834)). Therefore, according to a standard temperature-time curve (ETK), the glazings, including their frame and supports, must prevent the passage of flames and fire gases for at least 30 or 60, 90 or 120 minutes, to be assigned to categories G30, G60, G90 and G120. Similar regulations apply to classifications F30, F60, F90 and F120. In addition, in the fire resistance class F, the glass must not heat up on average by more than 140 ° C above the initial temperature, on its far side of the fire.
[0003] Fireproof glazings made of hardened alkaline borosilicate glasses are already known, which are commercially available for the fire protection classes G and F. These have a linear linear thermal expansion coefficient of, for example, 3.3 x 10-6 K-1. This low coefficient of linear linear thermal expansion reduces the thermal stresses in the glass occurring in the event of a fire, so that such glasses provide longer fire resistance times with lower edge shrinkage. However, these glasses have the disadvantage that because of the low coefficient of linear linear thermal expansion, only a very low quenching can be applied to these glasses on conventional air quenching plants, so that these glasses do not meet in general not to the requirements for safety glasses, such as the aforementioned DIN 1249. For this reason, alkaline borosilicate glasses have already been developed which have a coefficient of thermal expansion greater than 3.5 x 10-6 K-1. Such glasses are described for example in DE-A-42 30 607. The disadvantage of these glasses lies in the necessary content of ZrO 2. For example, it has been found that because of unmelted ZrO2 residues, these glasses tend to break spontaneously when tempering glass. DE-A-43 25 656 also discloses alkaline borosilicate glasses for fire protection glazings which meet the requirements for a thermally quenched fire safety glass. But these glasses also have disadvantages. For example, it has been found that with these glasses, during the forming process with the float process, the Zn2 + contained in the molten glass is reduced to Zn ° in the surface of the glass strip, due to the conditions. strongly reducing (partial pressure of oxygen p (02) in the float bath lower than 10-10 bar). However, the Zn ° evaporates easily, so that it separates from the glass by sublimation and condenses in the float bath on building elements such as assistance rollers, so that they must be regularly cleaned during the process, which is a complex operation. On the other hand, the non-sublimated but nevertheless reduced Zn forms a deposit on the surface of the flat glass, which strongly affects the quality of the glass. Furthermore, this type of glass necessarily contains ZrO 2 which, as mentioned above, has the disadvantage, in the case of fire-resistant glasses, that small amounts of non-molten ZrO 2 / ZrSiO 4, or ZrO 2 / ZrSiO 4 formed during a secondary crystallization, already lead to spontaneous breaks during the thermal quenching. In addition, Zr02 impairs melting behavior, resulting in significantly higher energy costs. DE-A-1995 15 608 discloses an alkaline borosilicate glass with a linear coefficient of linear thermal expansion of 3.9-4.5106-K-1. This glass is particularly suitable for fully electric melting under cold vault conditions.
[0004] However, for this glass, ZrO 2 is also an indispensable component, so that for the reasons mentioned above, it is not optimally adapted as a fire safety glass. DE-A-27 56 55 also discloses thermally toughened glasses with an expansion in the range of 3.39 '10 -6 K-1 to 5.32' 10 -6 K-1. . These glasses have the disadvantage of an intentionally high coefficient of thermal expansion, higher than the transformation temperature. This creates problems for dimensional stability under thermal stress, for example when coating at temperatures below the processing temperature but close to it. DE-A-44 30 710 discloses glasses with high chemical resistance. However, these glasses are difficult to melt and have a high density. EP-A-0 576 362 discloses a thermally stable and chemically resistant alkaline borosilicate glass for fireproof glass. However, it has the disadvantage of not being able to be subjected to thermal quenching on conventional air quenching plants, because of the high transformation temperature,> 600 ° C, and given the low viscosity in the range of melting temperatures (1 g (q / cP) = 2 to about 1450 ° C), a large number of refining agents, such as NaCl and KCl, can not be used. This also applies to JP-A-61 024 344, which also has a melting temperature which is too low for refining with sodium chloride. Moreover, the fraction V205 necessarily present is disadvantageous for forming by the float process, since the V5 + ion is reduced in the float bath. In addition, V205 has serious drawbacks for the desired high light transmission. Finally, US-A-5,776,844 discloses an alkaline borosilicate glass having good fire and thermal shock resistance. However, the coefficient of linear thermal expansion is between 8.0 x 10-6 K-1 and 9.5 x 10-6 K-1, and the strain point is only 25 K greater than that of normal soda-lime glass. On the other hand, the glasses have a low content of 5iO 2. Glasses of this type often have relatively low chemical resistance compared to higher alkoxilic borosilicate glasses.
[0005] DE-A-196 43 870 describes alkaline borosilicate glasses which are subjected to chemical quenching by ion exchange. The possible field of application of special glass induction hobs is described in JP 2003-086337 A, JP 2003-217811 A, WO 2003/098115 A1, DE 102 43 500 A1, DE 101 22 718 C2, DE 101 50 884 A1, DE 103 551 60, GB 2 079 119 A, US 6051821 A, WO 2004/018944 A1, and WO 2012/146860 A1. Other documents falling within the scope of the invention are the following: 37 22 130 A1, DE 40 122 88 Cl, EP 0 588 000 Bi, WO 96/33954 A2, JP 83145637 A, JP 89093437 A, SU 1284959 A, DE 44 28 235 C1, DE 1496637 A, FR 2389582 Al, JP It is an object of the invention to overcome the drawbacks and problems described above and to propose a borosilicate glass which can be used in the present invention. suitable for applications with high thermal stress, eg in the household sector, as glass for pyrolysis furnaces, as induction hobs, as functional glass in appliances microwaves, as glass for fire-resistant glazing, for applications with high mechanical stress, as glass for glazing without putty, as glass for anti-ballistic glazing, for structural elements with high static resistance in the field of building. The glass must then be designed in such a way that it is not necessary to subject it to thermal or chemical quenching to meet the strength requirements. Therefore, a material having a heat resistance of at least 400 ° C is required. The resistance of the material must be sufficiently high and the thermal expansion sufficiently low, so as to exclude a rupture due to induced thermal stresses during a period of use of several years of the product. On the other hand, the resistance requirements of the standards in this area (eg EN 60335) must be met.
[0006] It is desired to have a material which is otherwise transparent, with a very low inherent coloring. On the other hand, it is desired to obtain a material which also has a very good chemical resistance to acid (produced for example by food contaminants) and to the attack of alkaline detergents (due for example to the application of of cleaning). In addition, the glass must also meet the requirements for a fireproof glass. It should also be possible to decorate this material with coatings on its upper and / or lower side, so that the requirements listed above are fulfilled also for the coatings during the lifetime of the apparatus. Finally, it should be possible to easily melt the glass in all conventional pond installations and to seamlessly change the glass from Duran / Pyrex glass type to glass of similar density glass according to the invention, without draining the basin. The forming must be possible by rolling, floating, "up draw" or "down draw". The materials having the properties mentioned above were found with special alkaline borosilicate glasses and special lithium aluminosilicate glasses. The use of alkaline borosilicate glasses for this application has already been described by GB 2,079 11 A, but it is known that the described materials, having for example the composition comprising 81.1% SiO 2, 3.0% Na 2 O, 13.5% of B203, 2.2% of Al2O3 and a coefficient of expansion of 3.3 x 10-6 K-1 at 4.0 x 10-6 K 'can be quenched in quenching plants. This is the only way to meet the mentioned requirements for heat resistance and strength. This also applies to the glasses described in WO 2012/1468600 A1. In the absence of subsequent thermal or chemical quenching, the surface resistance of the glass elements is too low. These requirements are also not satisfied by other borosilicate flat glasses.
[0007] Solution of the problem The purpose mentioned above is achieved by the subject of the independent claims. Advantageous improvements of the invention are set forth in the respective independent claims.
[0008] In general, to solve the problem, use is made of an alkaline borosilicate glass having the following composition: 5O 2 70 - 86 wt.% Al 2 O 3 O - 5 wt.% B203 9.0 - 25 wt. 5.0% by weight K 2 O - 1.0% by weight Li 2 O - 1.0% by weight, as well as 0 - 5.0% by weight of other constituents.
[0009] Given the generally good chemical resistance of conventional alkaline borosilicate glasses, the proposed solution seeks above all to reduce the fragility of glass compared to known glasses such as Borofloat 33. According to another aspect of the invention, one of the Objectives is also to increase the intrinsic resistance. In addition to these two objectives, yet another aspect of the invention aims to obtain a not too high melting temperature. For this purpose, the following theoretical reflections and calculations correlate resistance properties and physical parameters of the glass substrates. The first of these reflections establishes a relation between the intrinsic resistance and the coefficient of thermal expansion, which proves to be surprisingly correct compared to the experiment, as regards the order of magnitude as the expected trend. The result is approximately an inverse proportionality between the intrinsic resistance and the coefficient of thermal expansion, so that for example the lowering of the coefficient of thermal expansion, the value of Borofloat 33, that is to say 33%. 7 1 (-1, at a value of less than 10%, ie 30 '10-7 K-1, leads to an increase of about 10% in the intrinsic resistance.) The second reflection establishes a relationship between The average weighted number of stress conditions is combined with the composition by a linear function in which tabular values and binding forces are also involved. second condition which, starting from a desired reduction in brittleness, results in an appropriate composition range, through an increase in the average weighted number of constraint conditions per atom. A third condition is derived from the desired maximum melting temperature. The reflections described above in general and the invention will be explained in detail hereinafter. Concerning the resistance, the intrinsic resistance is first considered, as specified above, by which is meant, in the sense of the invention, the strength of the material when it has just been produced. Measurements of this magnitude can be made for example on freshly drawn glass fibers. This intrinsic strength is also critical in use, if, after manufacture, the glass surface is protected against micro-deterioration by a suitable coating or, in general, by a surface treatment.
[0010] It is shown below that the intrinsic strength is decisively influenced by the coefficient of expansion, so that the objective of providing an alkaline borosilicate glass as resistant as possible is achieved by an alkaline borosilicate glass having a suitable coefficient of expansion (as low as possible, as we will see below). According to H. Fôll, notes for the lecture "Einführung in die Materialwissenschaft I" (Introduction to the science of materials), Christian Albrechts-Universität of Kiel, the limit of the intrinsic resistance is reached when the atoms have been removed until at the point of inflection of the interatomic potential. The interatomic potential U (r) can be described for example by a Morse potential. For simplicity, the examination is limited to interactions in the direction of the constraints, and the transversal effects are neglected. As a result, the square-column structure can be divided with the area of section r02, where ro is the equilibrium distance of the atoms. A break occurs when the force applied from the outside adopts, by atomic column, the absolute value of the derivative of U at the point of inflection WP of the potential, which means that the externally applied voltage is deemed to be equal to the negative derivative divided by ro2: 1 (dLP kritisch 2 dr ro a y vvp For the other calculations, U is developed around the position of equilibrium ro in a series of Taylor of third order, x = r - ro: 1 1 U »U0 + -U0 - x2 + -U0 - x3 + 2 6 It is remarkable that the different orders of the Taylor series or the different derivatives of U in ro are combined essentially with different physical quantities, namely the second derivative. with the modulus of elasticity and the third derivative 25 with the coefficient of thermal expansion, both of which will be discussed below, with the aim of ultimately obtaining the relationship between the critical voltage, and thus the intrinsic resistance, and the coeffici In order to give a positive thermal expansion, the third Uo'n derivative of the potential must be negative. The details of this relationship will be described later. According to the conference notes cited above: (1) 15 (2) (3) (10 'E - ro E denotes the modulus of elasticity and ro' the volume per atom.
[0011] The invention is based on the discovery that the coefficient of thermal expansion can be noted as follows: (4) 110 2 = 2 hp P-ro 6.1.1; The above conference notes use a simplified relation that uses the Boltzmann constant "k" for specific heat per atom and dimension. On the other hand, equation (4) calculates, according to the invention, with (c, 'p' 1-03 / 3), where c, is the specific heat per unit weight, p the density and ro 'the volume assigned to an atom. (The factor 1/3 results from the fact that c, depends on vibrations in the three spatial directions, but here only one direction is decisive). This relation is also consistent with the relationship, named after Grüneisen, between the coefficient of thermal expansion and the specific heat (see also for example NL Vaadlo, Geoffrey D Price, The Grüneisen parameter - computer calculations via lattice dynamics, Physics of the Earth and Planetary Interiors, 82 (1994) 261-270). With regard to intrinsic resistance, the invention is based on the discovery that the foregoing equations can be combined to establish a relationship between the resistance, respectively the critical stress and the associated coefficient of linear thermal expansion. For the critical stress, it follows in accordance with the invention: ## EQU1 ## (5) G kritisch-2 r = -2 U0-X-1 Uo-X2 = It is remarkable that the critical stress depends in this approximation only on the specific heat per volume (c, p) and the coefficient of expansion, the quality of this approximation depends on the precision with which it is applied. can determine the position of the inflection point of the potential curve, when the potential curve is described by a third order Taylor series around the equilibrium position This exact description does not exist for very small coefficients hence the singularity for a = 0. However, for a coefficient of expansion close to 10 ppm / K, a value of remarkable quality is obtained, if we consider as an example embodiment of soda-lime glass (coefficient of dilation 9 ppm / K, specific heat 720 J / kgK), density 2,500 kg / m3, see "Mechanische und physikalische Eigenschaften von Kalk-Natron-Silikatglas und von Borosilikatglas nach EN 572-1 [64] und EN 1748-1 (61)", www.baunetzwissen.de), this results in a critical stress of about 16 GPa, which is of the order of magnitude of intrinsic resistances observed, cf. C.R. Kurkjian, P.K. Gupta, R.K. Brow, N.
[0012] Lower, 'The intrinsic strength and fatigue of oxide glasses', Journal of Non-Crystalline Solids 316 (2003) 114-124.The advantage of the approximation described here lies in the fact that it clearly shows the relationship between resistance intrinsic and coefficient of expansion This is not contained in the usual approximation, see Egon Orowan, 'Die mechanischen Festigkeitseigenschaften und die Real struktur der Kristalle', Zeitschrift Kristallographie, (A) 89 (1934), 327-343 , and commentary on this article in Prabhat Gupta, 'Strength of Glass Fibers', in M. Elices and J. Llorca (Editors), 'Fiber Fracture', Elsevier Ltd., 2000, ISBN: 978-0-08- 044104-7. This result is also consistent with observations made in experiments, according to which the intrinsic resistance of silica glass, which has a very low coefficient of expansion, is high compared to other glasses, cf. C.R. Kurkjian, P.K. Gupta, R.K. Brow, N. Lower, The intrinsic strength and fatigue of oxide glasses, Journal of Non-Crystalline Solids 316 (2003) 114-124.
[0013] Therefore, if a high intrinsic strength glass is sought in a glass family in which the specific heat per volume changes little, the expansion coefficient of the glass is lowered according to the invention by changing the composition, or else selects glass compositions that have as low expansion coefficients as possible. For the purposes of the invention, borosilicate glass, which is as resistant as possible, means a glass whose intrinsic strength is further increased compared to a commercial Borofloat 33 glass. From the foregoing explanations, this is specifically a borosilicate glass whose coefficient of expansion is decreased compared to Borofloat 33. A reduction in the coefficient of expansion of 10% corresponds to a 10% increase in intrinsic resistance. The fact that the decrease of the coefficient of thermal expansion also reduces the thermal stresses occurring in the presence of temperature gradients constitutes an additional effect which corresponds to the object of the invention. The coefficient of expansion is hereinafter referred to the temperature value 210 ° C. for which there is a very precise regression function, cf. Alexander Flügel, Thermal Expansion Calculation of Silicate Glasses at 210 ° C, Based on the Systematic Analysis of Global Databases, http://glassproperties.com/expansion/Expansivity Glass 2006.pdf. Regarding the coefficients for the different glass components presented in tabular form, this document is also incorporated in its entirety in the subject of the present invention. This regression function is as follows (for a in ppm / K): ## EQU1 ## , Ck are the molar concentrations (in mole percent) of the respective components of the glass composition.
[0014] The coefficients 13e, Bi, Bi2, Bik associated are the following: Coefficient Value Axis portion (PO 1.7672 Na2O (13D 0.4545 Na2O (Be) -0.001198 Ca ° (13D 0.1682 Al2O3 (13D -0.0641 A1203 (13i2) 0.006473 K20 ( 13D 0.5320 1 (20 (13i2) -0.001710 MgO (op 0.0499 B203 (13D 0.0465 Li20 (13D 0.1896 Li20 (Be) 0.003242 Sr0 (13D 0.1717 BaO (O)) 0.3077 ZrO2 (op -0.0591 TiO2 (13i) -0.0138 ZnO (op. 13D 0.0102 Pb0 (13D 0.1345F (PD 0.1305 Na2O * Ca0 (13I1) -0.002579 Na2O * B203 (13I1) -0.005640 Na2O * Li2O (13I) 0.018869 CaO * MgO (P1) 0.002627 CaO * B203 (13I2) -0.002682 CaO * Ba0 (13ik) -0.011958 K20 * B203 (13ik) -0.012682 As an exemplary embodiment for calculation with the regression formula, a borosilicate glass having the known composition of Borofloat 33, namely 81% by weight, is first considered. of SiO 2, 12.5% by weight of B 2 O 3, 2.5% by weight of Al 2 O 3, 3.5% by weight of Na 2 O, 0.5% by weight of K 2 O, i.e., converted to% molar, 83.53 mol% SiO 2, 11.12 mol% B 2 O 3, 1.52 mol% Al 2 O 3, 3.5 mol% Na 2 O, 0.33 mol%. of K20). Then, at 210 ° C, the glass has a thermal expansion of 3.69 ppm / K. In order to obtain an increase in the intrinsic strength with respect to this glass, the composition of the glass is modified, in accordance with the invention, so that there is a decrease in the thermal expansion. Since a significant reduction in thermal expansion is detrimental to the possibility of melting, this reduction must be carried out in small steps. For comparison: at the end of a subsequent reduction in thermal expansion, quartz glass is obtained with about 0.6 ppm / K at 210 ° C but with a melting point of about 2700 ° C. By melting point is meant here according to A. Flügel, Glass viscosity calculation based on a global statistical modeling approach, Glass Technol. Eur. J. Glass Sci. Technol. A, February 2007, 48 (1), 13-30, the temperature at which the viscosity is 10 ** 1.5 pascal-second. For quartz glass practically free of water according to M.L.F. Nascimento, E.D. Zanotto, Diffusion processes in vitreous silica revisited, Phys. Chem. Glasses: Eur. J. Glass Sci. Technol. B, Aug. 2007, 48 (4), 201-217, this point can be evaluated at about 2700 ° C.
[0015] Therefore, according to one embodiment of the invention, therefore, alkaline borosilicate glasses are selected in the composition range, indicated above, with 70-86% by weight of SiO 2, 0-5% by weight of Al 2 O 3. , 9.0 - 25% by weight of B203, 0.5 - 5.0% by weight of Na2O, 0 - 1.0% by weight of K20, 0 - 1.0% by weight of Li2O, as well as 0 - 5.0% by weight of other constituents, a composition for which the thermal expansion at 210 ° C according to equation (17) is at most 3.6 ppm / K, preferably at most 3.5 ppm / K, particularly preferably at most 3.4 ppm / K, especially at most 3.3 ppm / K.
[0016] To achieve high intrinsic strength, even lower expansion coefficients can be achieved by selecting the glass components. The coefficient of linear thermal expansion may especially be at most 3.2 ppm / K, preferably at most 3.1 ppm / K, particularly advantageously at most 3.0 ppm / K. The invention is also based on the fact that the fragility can be attributed approximately to the composition, and this through a weighted crosslinking index. According to the invention, the force which is necessary to produce a permanent depth impression ("dimpling", see Trevor Wilantewicz, ARL-TR-5180 Army Research Laboratory Report, May 2010) can also be attributed to the index. weighted crosslinking. Fragility can be defined in the sense of J. Sehgal, S. Ito, Brittleness of glass, Journal of Non-Crystalline Solids, Volume 253, Editions 1-3, August 1999, pages 126-132 or the c / a value ( ratio between the average radial-median crack length and the half-width of the indenter) which is equivalent in the case of a fixed test force value. The c / a value is almost a measure of the normalized distance at which the deterioration stops with respect to the center of deterioration, cf. Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005, the entire contents of which are included in this specification, with respect to the determination of c / a values. disclosed in this document, as well as their size. The invention provides a method for determining such a crosslinking index and for selecting suitable glasses with low brittleness. The state of the art prior to the invention is essentially described, for example, in P. Boolchand, 'Intermediate phases, reverse osmosis, stress-free and non-aging networks, and strong liquids', Chalcogenide Letters Vol 3, No. 2, March 2006, pp. 29 to 31. According to this document, it is possible to evaluate important properties of the glass, if one determines the average number of stress conditions to which an atom is subjected in the vitreous network. a neighboring atom atom (= coordination), it follows from the conditions of distance r with respect to these neighbors r / 2 distance conditions to be assigned to this atom, if we distribute the distance conditions equally on the two partners It follows from the angles of connection between these neighbors, where the atom considered is at the tip of the respective angle, other conditions of angle 2r-3 which must be associated with this atom, see P Boolchand, MF Thorpe, Glass-forming tendency, per colation of rigidity, and onefold -component atoms in covalent networks ", Phys. Rev. B 50, No. 14 (1994), p. 10366-10368, as well as M.F. Thorpe, J. Non-Cryst. Solids 57, 355 (1983), H. He and F. Thorpe, Phys. Rev. Lett. 54, 2107 (1985). For a total number of three stress conditions, the number of stress conditions per atom is exactly equal to the number of degrees of freedom per atom, cf. There also P. Boolchand, F. Thorpe, 'Glass-forming tendency, percolation of rigidity, and onefold-contacted atoms in covalent networks', Phys Rev. B 50, No. 14 (1994), pp. 10366-10368. Such a material is called "rigid." If the number of constraint conditions per atom is less than 3, there are several possible configurations, that is, the glass has degrees of freedom of configuration. to pass to each other without energy input, according to the simple scheme developed here, in fact, they are slightly different in terms of energy.This system is referred to as "floppy" (flexible).
[0017] In addition to these two cases, there is the case of "over-constraint rigid" in which the number of the constraint conditions is greater than that of the degrees of freedom, and which can only be achieved by providing system energy to go against one or more conditions of constraint.
[0018] An example of a "rigid" system is silica glass. Admittedly, it seems at first that the number of constraint conditions per atom is greater than 3. Assuming that silicon has the coordination 4 and oxygen the coordination 2, we obtain a silicon atom 4/2 + 24-3 = 7 stress conditions, and per oxygen atom 2/2 + 2'2-3 = 2 stress conditions, and therefore an average number of stress conditions of 11/3 = 3.67 per atom. According to Zhang, P. Boolchand, 'The Central Role of Broken Bond-Bending Constraints in Promoting Glass Formation in the Oxides', Science, New Series, Vol 266, No. 5189 (1994), 1355-1357, the conditions concerning oxygen (which also correspond to the vitrification rules of Zachariasen, see WH Zachariasen, J. Am. Chem., Soc., 54 (1932), 3841) can be neglected, so that gives an average number of stress conditions of 9/3 = 3. Therefore, according to this reasoning, the number of degrees of freedom of configuration is zero, which is consistent with the extremely low temperature specific heat in the temperature range of the glass transition, see R. Brüning, "On the glass transition in vitreous silica by differential thermal analysis measurements", Journal of Non-Crystalline Solids 330 (2003) 13-22. (In fact, the number of degrees of freedom of configuration is not equal to zero, but very small). The aforementioned sudden change in specific heat reflects the "thaw" of the degrees of freedom of configuration of the glass which contribute to the specific heat at higher temperatures, ie higher than the glass transition. The importance of this sudden variation is a measure of the number of degrees of freedom of configuration, cf. Charles Austen Angell, Thermodynamic aspects of the glass transition in liquids and plastic crystals, Pure & Appl.
[0019] Chem., Vol. 63, no. 10, pp. 1387-1392, 1991 and M.L.F. Nascimentoa, C. Aparicio, Viscosity of strong and fragile glassforming liquids investigated by means of major component analysis, Journal of Physics and Chemistry of Solids 68 (2007) 104110.
[0020] We now examine multicomponent glasses that additionally contain aluminum, boron and alkali ions and optionally alkaline earth ions, with the restriction that the molar fraction of aluminum oxide is less than the sum molar fractions of the alkaline oxides, and possibly also alkaline earth oxides. In this case, it can be assumed that all the aluminum is present in a quadruple coordination with oxygen, cf. M. Bertmer, L. Züchner, J.C.C. Chan, H. Eckert, J. Phys. Chem. B 104 (2000) 6541, J.C.C. Chan, M. Bertmer, H. Eckert, J. Am. Chem. Soc. 121 (1999) 5238, L. Züchner, J.C.C. Chan, W. Muller-Warmuth, H. Eckert, J. Phys. Chem. B 102 (1998) 4495, and a corresponding fraction of sodium ions is distributed without bond in the vitreous network. This results first of all for the corresponding aluminum atoms (as above for the silicon atoms) in each case 2 distance conditions and 5 angle conditions, and for the corresponding oxygen atoms (a part of which has was "taken" on alkaline oxides or alkaline earth oxides) each time 1 condition of distance. (As before, the angle conditions for oxygen are neglected).
[0021] On the other hand, according to the invention, only alkaline borosilicate glasses are used according to the composition range indicated above, in particular alkaline borosilicate glasses which contain as cations exclusively silicon, boron, aluminum and alkaline and / or alkaline earth metals. In addition, alkaline borosilicate glasses are examined in which the difference in the sum of all the alkali oxides, if appropriate also alkaline earth oxides, and A1203 (in mole percent) is less than 0.7 times the fraction of B203 (in molar percent). In this case, for all the compositions which are "alkaline borosilicate glasses" according to the above definition, and with a technical cooling, it can be assumed that the molar percentage of B 2 O 3 converted to boron with 4-fold coordination with oxygen corresponds to the difference quoted, cf. YH Yun, PJ Bray, "Nuclear magnetic resonance studies of the glasses in the Na20-B203-5152 system", J. Non-Cryst Solids 1978, 27, 363-380, WJ Dell, PJ Bray, SZ Xiao, "B NMR studies and structural modeling of Na20-B203-Si02 glasses with high soda content ", J. Non-Cryst Solids 1983, 58, 1-16, Hiroshi Yamashita, Kazuhiko Pout, Takeshi Nakajin, Hyuma Pout, Takashi Maekawa," Nuclear magnetic resonance studies of 0,139M0 (or M'20) - 0,673Si02 - (0,188-x) A1203 - xB203 (M = Mg, Ca, Sr and Ba, M '= Na and K) glasses ", Jingshi Wu, Jonathan F Stebbins, "Temperature and modification cation field strength effects on aluminoborosilicate glass network structure", Journal of Non-Crystalline Solids 362 (2013) 73-81 For boron atoms which are then brought to the quadruple coordination and for the atoms of associated oxygen (some of which has been "removed" from alkaline oxides or alkaline earth oxides), 3 stress conditions per atom apply, as above for silicon and aluminum with quadruple coordination. For the remaining boron atoms, which are triple-coordinated, cf. Jingshi Wu, Jonathan F. Stebbins, "Journal of Non-Crystalline Solids 362 (2013) 73-81, and the associated oxygen atoms, there are 3 / 2 + 2.3-3 = 4.5 stress conditions per boron atom and 1 stress condition per oxygen atom, ie on average (9 + 3) / 5 = 2.4 stress conditions per atom. With regard to the alkaline ions and the alkaline earth ions, it is at first uncertain on what number of neighboring oxygen atoms is based, because with a mainly ionic bond, the coordination is not necessarily equal to the valence. However, if we agree with Zachariasen, who requires for vitrifiable systems that the coordination of oxygen is always "2", it must be assumed, in order to obtain electrical neutrality, for alkalis, a neighboring oxygen and the alkaline-earths two adjacent oxygens, so that for the alkaline and alkaline-earth oxides respectively two distance conditions result, and consequently 2/3 stress conditions per atom for the alkaline oxides and 1 condition of stress by atom for alkaline earth oxides. Angle conditions are not calculated for alkaline and alkaline earth metals because of the mainly ionic bond. For a system in the composition range indicated above, a mean number of stress conditions per atom can now be calculated directly, via the molar mixing ratio, by dividing the number of stress conditions for one mol. of the respective composition by the number of atoms.
[0022] This average number of stress conditions per atom can be considered as crosslinking index, because the number of constraint conditions per atom is even higher than the atoms are crosslinked with each other. The approach according to which the Vickers hardness increases proportionally to an increasing average number of stress conditions per atom is also known, cf. Morten M. Smedskjaer, John C. Mauro, Randall E. Youngman, Carne L. Hogue, Marcel Potuzak, and Yuanzheng Yue, 'Topological Principles of Borosilicate Glass Chemistry', J. Phys Chem B 2011, 115, 12930-12946 However, in this publication, the procedure is different in two respects from the method according to the invention: the angle conditions for oxygen are counted for the calculation of the hardness, the alkalis or the alkaline earth, where "oxygen" has been "removed" from aluminum or boron, are not considered to be constituents of the network and are not counted for the calculation of the number of stress conditions per atom. according to the aforementioned publication, there are two additional stress conditions for all alkalis where oxygen has not been "removed" from aluminum or boron, because of the tendency to group alkalis. does not conflict with the method according to the invention because among the compositions according to the invention, there are none where the oxygen has not been completely removed alkali or alkaline earth. According to the aforementioned publication, Morten M. Smedskjaer, John C. Mauro, Randall E. Youngman, Carne L. Hogue, Marcel Potuzak, and Yuanzheng Yue, 'Topological Principles of Borosilicate Glass Chemistry', J. Phys Chem B 2011, 115, 12930-12946, the following formula is used: (7) Hv = const - (n-2.5) where H, is the Vickers hardness, n is the average number of stress conditions per atom, and 2.5 is the lower limit found by the authors for a "hard" metal In the glasses they studied, the authors found in the SiO2-B203-CaO-Na20 system the confirmation of the postulated relationship (7). However, this method can not be easily applied to the fragility referred to herein, in the sense of the value c / a described above. <br /> <br /> This is where the invention comes into play.
[0023] While hardness is a measure of the resistance to deformation, the c / a value is based on a break. Since the macroscopic failure in all cases also includes the microscopic breaking of bonds, an expression that can be correlated with fracture toughness should include the bonding forces. For this purpose, in accordance with the invention, the stress conditions mentioned above are weighted with the binding forces. This concerns the two types of stress conditions, namely the angle conditions as well as the distance conditions. For the angle conditions, it is also necessary to take into account the proportion of ionic bond of the respective bond, which varies according to the cation that occurs. For this reason, weighting factors are introduced. Since the angle conditions are a consequence of covalent bonds, all angle conditions are weighted with a degree of covalence K which is defined as one minus the respective ionic binding proportion of the M-O bond (M = Si, Al, B, Alkaline, alkaline earth). This proportion of ionic bond can be interpreted as the probability that the binding partners are present in an ionized form. Conversely, the angle conditions are weighted, according to the method developed here, with the probability that the partners are present with a covalent bond. The proportion of ionic bond I of each single bond is calculated from Linus Pauling, "The Nature of the Chemical Bond," Cornell University Press, New York, 1960, from the difference in electronegativities, represented in tabular form in this document, anions (xA) and cation (xi (): (1,4-xK) 2 (8) -e 4 In view of the already known uniqueness of SiO 2 as a "strong glassformer" glass formation), see Charles Austen Angell, Thermodynamic aspects of the glass transition in liquids and plastic crystals, Pure & Appl., Vol 63, No. 10, pages 1387 to 1392, 1991, the glass classification Si02 should not be influenced, for this reason all degrees of covalence are normalized by dividing them by the degree of covalency of the Si-O bond, so it is no longer necessary to decide which bonds should be considered as predominantly ionic or mainly covalent. mainly ionic ison, the angle conditions for alkali and alkaline earth continue to be ignored in the calculations. Secondly, all the stress conditions, namely the distance conditions as well as the angle conditions, are weighted with the binding force of the respective single M-0 bond ("single bond strength"). . It is normalized by dividing by the bonding force of the simple Si-0 bond. For liaison forces, reference is made to V. Dimitrov, T. Komatsu, "An interpretation of optical properties of oxides and oxide glasses in terms of the electronic polarizability and average single bond strength (Review)", Journal of the University of Chemical Technology and Metallurgy, 45, 3, 2010, 219-250.
[0024] These binding forces have been calculated by dividing the dissociation energy ed for a cation by the number of oxygen atoms surrounding the cation, i.e. by the coordination. If we base ourselves on another coordination than that of Dimitrov and Komatsu, we must convert accordingly. This conversion does not affect the number of weighted distance conditions according to the method given here, because when calculating it, the coordination disappears with simplification. The number of distance conditions is r / 2, where r is the coordination (see above); the weighting factor is ed / r / link strength of the Si-0 bond, and therefore the weighted number of distance conditions for a cation with ed / 2 / bond strength of the Si-O bond is obtained. Therefore, it can generally be assumed that the coordination is equal to the valence of the respective cation; thus, the coordination of oxygen is always "2", in agreement with Zachariasen. The angle conditions are also treated judiciously. The angle conditions are valid only for the case (more and more unlikely as the difference in electronegativity with oxygen increases) where the cation has a covalent bond; now, in this case, the coordination is in general equal to the valence. Exceptions are cations which can effect a coordination change and show a mainly covalent bond also in the new coordination (by hybridization), namely boron and aluminum. We then proceed as described above. For the sake of simplicity, it is possible to relate all the conditions of distance to the cations, and the total number N of the stress conditions per mole is then obtained (as explained above, only the case where the mole fraction of aluminum is less than the sum of the molar fractions of the alkaline oxides, if appropriate by adding the alkaline earth oxides, where the cations present are only silicon, boron, aluminum and alkalis and / or alkaline earths , and where the difference of the sum of all the alkaline oxides, where appropriate by adding the alkaline earth oxides and A1203 (in mole percent) is less than 0.7 times the fraction of B203 (in mole percent): (9) N - = c (SiO 2) - 9 NA (IC (B - O) ed (I 3 - O) 1 4 IC (Si - O) 1 ed (Si - O) 1 4 MA 1 --Or ed (A1 - 0) 14 + c (A1203) - 2. 4 + 5 ((- 0) ed (Si-O) 1 4 2- 3 + 3.IC (13-ed (13-0) 13 ((- ( + Ic (M; 0) + Ic (M 0) - c (A1203) - 2. 4 + 5 (- 0), ed (Si-O) 14 + c (B2o3) + c (At2o3) - lek) -Ic (mio) + c (M0) 2 ed, (Ml edO'i f 4 + 1cM-'0) 2 e -0) 12 d Here, c are the molar concentrations, the alkali and Mi the alkaline earths. K (M-0) are the covalent degrees of the respective M-O bond, ed (M-0) the respective dissociation energies, referred to a cation, and NA is the Avogadro number. The number n of the constraint conditions per atom results from N / NA, by dividing by the molar fractions of the different oxides which have been multiplied by the number of atoms per oxide and then totalized: (9b) n = c1Si021-3 + 4A / 2031-5 + c (13203) - 5 + 1c (A 1120). 3 + Ic (M-10) .2 ed (Si-0) / 4 Unlike Morten M. Smedskjaer, John C. Mauro, Randall E. Youngman, Carne L. Hogue, Marcel Potuzak, and Yuanzheng Yue, Topological Principles of Borosilicate Glass Chemistry ", J. Phys Chem B 2011, 115, 12930-12946, the oxygen angle conditions are not counted, but the alkaline or alkaline earth metals, to which oxygen has been removed by aluminum or boron, are taken into account for the calculation of the number of stress conditions per atom .. The degrees of covalence and the dissociation energies are presented below in tabular form for the oxides in question. The degrees of covalency are calculated from the electronegativities according to Pauling, Linus Pauling, The Nature of the Chemical Bond, Cornell University Press, New York, 1960, according to formula (8). In addition to the dissociation energies, taken either in V. Dimitrov, T. Komatsu, "An interpretation of optical properties of oxides and oxide glasses in terms of the electronic polarizability and average single bond strength (Review)", Journal of the University of Chemical Technology and Metallurgy, 45, 3, 2010, 219-250, or in Kuan-Han Sun, Fundamental Condition of Glass Formation, Journal of The American Ceramic Society 69, 1947, 277-281, are given values for the determination of which one has calculated the dissociation energies of the respective oxides as the sum of the standard formation enthalpies plus the enthalpies for the transition of the participating elements from the standard state to a monoatomic gas. The standard formation enthalpies as well as the enthalpies for the transition of the participating elements, from the standard state to a monoatomic gas, are shown in the table "Standard Thermodynamic Values at 25 ° C" on the website "http: // www. chemistryreference.comr which in turn indicates as sources Dean, John A., Lange's Handbook of Chemistry, llth ed., McGraw-Hill, New York, New York, 1979, pages 9: 4-9: 128 as well as Lide, David R., CRC Handbook, 84th ed., CRC Press, Boca Raton, Florida, 2003, pp. 5: 5 to 5:60, 5:85 to 5:86.
[0025] Oxide ed / (kJ / mol) ed / (kJ / mol) (eigenvalues) Degree of covalence (Dimitrov / Komatsu) Si02 1772 1864 0.5527 B203 1494 1572.5 0.6126 A1203 1506 1537 0.4329 Li20 600 585 0.2202 Na 2 O 4 070 02070 K20 500 395 0.1979 MgO 930 999 0.3216 CaO 1064 1063 0.2257 For comparison: Oxide ed / (kJ / mol) (Sun) ed / (kJ / mol) (own calculations) Degree of covalence Pb0 607 664 0.5104 The calculations shown below are based on the dissociation energies obtained by own calculations.
[0026] The average number of stress conditions per atom thus determined constitutes the desired weighted crosslinking index. For pure silica SiO 2 glass, the result is, after construction, the weighted crosslinking index "3". For Pyrex® with the composition of 81 mol%. SiO 2, 13 mol% of B203, 2 mol%. of A1203 and 4 mol%. Na 2 O, cf. Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005, results in a weighted cross-linking index of "2,883". For pure borate glass B203, a weighted cross-linking index "2,845" results.
[0027] For float glass with the composition 70.3 mol%. 0.52, 0.4 mol%. of A1203, 9.3% mol. CaO, 6.1 mol%. of MgO, 13.7 mol%. Na 2 O, 0.1 mol%. of K20, cf. Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005, first obtained a weighted cross-linking index "2,449". If one calculates in the manner of Morten M. Smedskjaer, John C. Mauro, Randall E. Youngman, Carne L. Hogue, Marcel Potuzak, and Yuanzheng Yue, 'Topological Principles of Borosilicate Glass Chemistry', J. Phys. Chem B 2011, 115, 12930-12946, it is appropriate to count, for all the alkalis to which oxygen has not been withdrawn and which are therefore part of the network in the sense of Smedskjaer et al., Two additional conditions of stress because of the tendency to group alkalis, this concerns 13.4 mol% of Na 2 O. (It must be assumed that the transition of aluminum atoms to tetrahedral coordination by incorporation of oxygen atoms alkaline and alkaline-earth oxides, is at first at the expense of the atoms of potassium, because among all the atoms of alkalis and alkaline earths, they have the weakest binding enthalpies, see the table In a similar way, this transition takes place in the second at the expense of sodium atoms. The transition is complete, that is to say that with a sufficient supply of alkalis, all the aluminum atoms go to the quadruple coordination, cf. B.H.W.S. DeJong, C.M.Schramm, and V. Eparziale, Polymerization of silicate and aluminate tetrahedra in glasses, melts, and aqueous solutions - IV. Aluminum coordination, Geochimica and Cosmochimica Acta vol. 47, 1983, 1223-1236. The problem of avoiding Al-O-Al bonds does not arise in view of the small amount of aluminum present. For the transition of 0.4 mol%. from A1203, the 0.1% K20 present is fully used. On the other hand, 0.3% mol is used. of Na 2 O, so that 13.4 mol% remain. as Na 2 O 2). This results in 2 * 2 * 0.134 moles = 0.536 moles of additional stress conditions per mole of oxides. The 0.506 mole of additional stress conditions per mole of oxides is weighted with the factor ed (Na-O) / (ed (Si-O) / 4). Each mole of oxides contains 0.703 * 3 moles of 512 atoms, 0.004 * 5 moles of A1203 atoms, 0.093 * 2 moles of CaO atoms, 0.061 * 2 moles of MgO atoms, 0.137 * 2 moles of Na 2 O atoms and 0.001 * 2 moles of K 2 O atoms, i.e., a total of 2,851 moles of atoms. Per atom, this results in 0.1777 additional stress conditions, so that the weighted crosslinking index for the float glass considered here is 2.626. For the calculation of the weighted crosslinking index of a high-lead glass, with the composition 13% mol. SiO 2, 6 mol%. of A1203, 22 mol%. B203, 58 mol%. of Pb0, cf. Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005, it is first necessary to have indications regarding coordination etc. aluminum, boron and lead; for the latter, this indication also relates to the changing character as network trainer or network modifier. While Pb2 + in small molar fractions acts as an ion-bound network modifier and transfers oxygen to the aluminum or boron, allowing the tetrahedral coordination of these atoms, the covalent bond is preponderant for important molar fractions, cf. A. Sawvel, S. Chinn, W. Bourcier, R. Maxwell, Local Structure of Amorphous (Pb0) '[(B203) iz (A1203) 1y (SiO2) Dielectric Materials by Multinuclear Solid State NMR, Lawrence Livermore National Laboratory, UCRL -JRNL-200058, 9.9.2003. In the range of 60 mol%. of Pb0, the fraction of boron atoms present in tetrahedral coordination decreases to about 1/3 and, in PbO-B203-Al2O3-5iO2 glass, to almost zero, if the aluminum supply is sufficient, because when switching to tetrahedral coordination, aluminum is preferred to boron, cf. A. Sawvel, S. Chinn, W. Bourcier, R. Maxwell, Local Structure of amorphous (Pb0) x [(B203) 1-z (A1203) 4y (5i02) and Dielectric Materials by Multinuclear Solid State NMR, Lawrence Livermore National Laboratory, UCRL-JRNL-200058, 9.9.2003. Therefore, for the composition of a lead-rich glass, which is present at Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005, one can start from principle that without the simultaneous presence of aluminum oxide, about 1/3 of the 22 mol%. from B203 to tetrahedrally coordinated boron, but due to the presence of 6% mol. of A1203, virtually no boron but all of the aluminum is tetrahedrally coordinated. For this purpose, 6 mol%. of Pb0 are "consumed", which are ionically bonded. The 52% mol. remaining are covalently bound. The covalently bonded Pb 2 + is present in the glass in a triple or quadruple coordination, cf. T.
[0028] Takaishi, J. Jin, T. Uchino, and T. Yoko, Structural Study of Pb0-B203 Glasses by X-ray Diffraction and "B MAS NMR Techniques, J. Am., Ceram Soc., 83, 2000, 2543-48. For lead borate glasses, of which, due to the small fractions of 5iO 2 and Al 2 O 3, the high-lead glass indicated by Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred, is an approximation. University, Alfred, NY, USA, 2005, authors T. Takaishi, J. Jin, T. Uchino, and T. Yoko, Structural Study of Pb0-B203 Glasses by X-ray Diffraction and "B MAS NMR Techniques, J. Am. Ceram. Soc., 83, 2000, 2543-48, indicate triple coordination; and also for the associated oxygen, which maintains the charge neutrality. Correspondingly, when calculating the angle conditions, the 52 mol%. of covalently bound lead are counted as having a covalent triple bond, while there are no angle conditions for the 6 mol%. lead ionic bond. The angle conditions on oxygen, for which the rules of Zacharias are here broken, are also neglected. The lead-rich glass thus has a weighted crosslinking index of 2.23 and is therefore significantly lower than the other glasses mentioned, which is primarily due to the very low ed value of Pb0, compared to CaO. Comparing the weighted crosslinking indexes, calculated here for the selected glasses, with the c / a values of Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005 there is a good correlation "high weighted crosslinking index - low c / a value (i.e., low fragility)". Glasses with a high weighted crosslinking index (silica glass, Pyrex® and pure borate glass) are part of the head group with regard to the c / a value, the float glass considered here belongs to the middle group, and the High lead glass is one of the most fragile glasses. For the three glasses of silica glass, Pyrex® and pure borate glass, exactly the same order is obtained if the decreasing weighted crosslinking index is calculated using the c-value. / a growing. The c / a value refers to the load exerted with a Vickers indenter and a load of 1 kg. Glass Value Index c / a (Wilantewicz) weighted crosslinking Silica glass 3 1.58 PyrexE 2.883 1.78 Pure borate glass 2.845 2.13 Float glass 2.626 2.89 Lead glass 2.23 4.49 the same hierarchy between silica glass, borosilicate glass and float glass (soda-lime) is obtained in relation to the intensity of the force required to produce a permanent depth impression ("dimpling", see Trevor Wilantewicz, Army Research Laboratory Report ARL-TR-5180, May 2010. The threshold at which the phenomenon of "dimpling" was observed for all the samples studied, applying a charge with a spherical indenter, was 100 N for silica glass, 35 N for borosilicate glass and 30 N for soda-lime float glass Here, the borosilicate glass was not Pyrex® but Borofloat 33® with a composition, in weight percent, of 81% 5iO 2, 12 , 5% B 2 O 3, 2.5% Al 2 O 3, 3.50% Na 2 O and 0.5% K 2 O, i.e. a molar composition of 83.53% SiO 2, 11.12% B 2 O 3, 1.52% Al 2 O 3, 3.50% Na 2 O and 0.33% K 2 O, and a weighted crosslinking index of 2.893. The soda-lime float glass was in this case Starphiree with a composition, in weight percent, of 73.2% SiO 2, 14.7% Na 2 O, 10.28% CaO, 1.44% Al 2 O 3 and other fractions for in total less than 0.5%, which are neglected, cf. Advances in Ceramic Armor VIII: Ceramic Engineering and Science Proceedings, Volume 33, Issue 5, 2012, edited by J. J. Swab, Volume editors M. Halbig, S. Mathur, Wiley, Hoboken, NJ, USA. This composition corresponds, in mole percent, to 73.43% 5iO 2, 14.29% Na 2 O, 11.05% CaO, 0.85% Al 2 O 3. In a similar manner to the float glass (sodocalcic) described above, of different composition, the weighted crosslinking index is calculated at 2.67. For the purposes of the invention, an alkaline borosilicate glass is understood to be as little fragile as possible, in particular a glass whose weighted crosslinking index, ie the average number of stress conditions per atom, is equal, according to formulas (9a) and (9b), more than 2.9, more preferably more than 2.91, particularly advantageously more than 2.92 and in particular more than 2.93.
[0029] Therefore, according to the invention, a high strength alkaline borosilicate glass comprising the following components is proposed: 5% 70 - 86% by weight Al 2 O 3 0 - 5% by weight B 2 O 3 9.0 - 25% by weight Na 2 O , 5 - 5.0% by weight K20 0 - 1.0% by weight Li20 0 - 1.0% by weight, as well as 0 - 5.0% by weight of other constituents, where the proportions of the components are chosen such that the weighted crosslinking index, that is the average number n of the stress conditions per atom, defined by c (SiO 2) -3 + c (A / 203) -5 + c (B 2 O 3) -5 + Ic (M ') 20) .3 + Ic (M-10) .2 has a value greater than 2.9, preferably greater than 2.91, particularly preferably greater than 2.92, and most preferably greater than 2.93, where NA denotes the number of Avogadro and c (SiO 2), c (Al 2 O 3) and c (B 2 O 3) the molar concentrations of SiO 2, Al 2 O 3 and B 2 O 3, c (1 4120) denotes the molar concentrations of the alkaline oxides 1 4'20 contents and c (I 4'0) the molar fractions of alkaline earth oxides contained, and where the N / NA ratio is defined by C (SiO 2) - 9 7 K (Al-0) ed (Al-O) 14 + c (Al 2 O 3) - 2-4 + 5 - K (Si - 0) e (Si - 0) 14 ' c (/ R0) +1 c (1 / I' 0) - c (Al 203) - 2-4 + 5- K (B - ed ( B - 0) 14 K (Si - e (Si - O) 14 '(B203) + c (Al 203) -1 4110) -14U' O) - 2- 3 K (B-O) ed (B) - 0) 13 + 3 K (Si - 0e (Si - 0) 14 +141 / 10) 2 ed (M '- O) e - 0) 14 +1 c (11/1' 0) 2 ed ( Where K (M-0), M = Si, Al, B, are the covalent degrees of the respective M-O bonds of the components 5iO 2, Al 2 O 3, B 2 O 3, and where ed (M-0) are the respective dissociation energies, referring to a cation, 5iO 2, Al 2 O 3, B 2 O 3 components or alkaline oxides or alkaline earth oxides. According to a preferred embodiment, the glass furthermore has a coefficient of linear thermal expansion of less than 3.6 ppm / K at a temperature of 210 ° C, since, as shown above, even low thermal expansion, generally increases the intrinsic strength of the glass. For the values of the dissociation energies ed (M-0) and the degrees of covalence of the components 5iO2, B20 and A1203, the values obtained by computation, represented in tabular form above, are particularly based. Correspondingly, a method according to the invention for making a glass element consists in selecting a N10 composition of a borosilicate glass, in the composition range indicated above with 70 to 86% by weight of SiO 2, which responds under the conditions of equations (20) and (21), with a value n greater than 2.9, and which at the same time has a coefficient of linear thermal expansion of less than 3.6 ppm / K at a temperature of 210 ° C, melting a glass having the determined glass composition, and forming a glass element from the molten glass. The glass elements made from the glass element manufactured in accordance with the invention are suitable for different uses where stability and heat resistance are of particular importance. Preferred uses are: - fire-resistant glazing, - façade elements, - heat protection glazing, in particular for cooking appliances or cooking ovens, as well as - glass pipe elements. As described above, the components of the glass are further preferably selected so that the regression formula (17) gives a linear thermal expansion coefficient a (210 ° C) of less than 3.6 x 10-6 K. -1. The composition of the glass therefore responds equally well to the demanding condition that the weighted crosslinking index, i.e., the average number n of the stress conditions per atom, indicated by equation (21), is greater than at 2.9, than that requiring the value of the regression formula (17) to be less than 3.6 '10-6 K-1. According to an improvement of the invention, the choice of the glass composition also takes into account the melting temperature. The melting temperature (in degrees Celsius) can also be calculated approximately using a regression formula.
[0030] This formula is as follows: ## EQU1 ## The coefficients CI, k, n also denote the various fractions (this time in percent by weight) of the glass components, and bikm are coefficients or weighting factors for these glass components. These factors are listed in detail in European Journal of Glass Science and Technology Part A Volume 48 Number 1, February 2007, the contents of which relate to the values shown in the table, as well as the aforementioned factors, are incorporated in their entirety into the object of the present invention. The coefficients 1) 0, b bik, bikm associated are the following: Coefficient Value 1) 0 1824,497 A1203 (bi) 19,341 B203 (bi) -22,347 B203. B2O3 (b) 0.60376 BaO (Bi) -18.931 Bi203 (Bi) -42.416 CaO (Bi) -17.453 CaO. CaO (bn) 0.12038 CeO2 (131) -22.418 Cl (bi) -8.563 CuO (bi) -30.913 F -11.739 Fe2O3 (bI) -13.611 K20 (131) -31.907 K20. K20 (bu) 0.61234 K20. K20. K20 (bill) -0.006662 Li 2 O (131) -30,336 Li 2 O. Li 2 O (bu) 0.22499 MgO (bI) -5.038 MnO 2 (b) -17,050 Na 2 O (b) -30,610 Na 2 O. Na 2 O (1) 11) 0.27887 Nd 2 O 3 (b) -39.662 PbO (b) -21,349 SO 3 (b) -13,908 SrO (b) -17,292 ThO 2 (1) 1) -17,185 TiO 2 (131) -10,323 UO 2 ( 1) -17,672 V205 (bi) -21,727 ZnO (bI) -6,280 ZrO 2 (1:11) 10,173 Al 2 O 3. Li 2 O (b) -0.38421 Al 2 O 3. Na 2 O (b) -0.23,085 Al 2 O 3. Mg0 (b) -0.44589 Al2O3. Ca0 (b) -0.93909 B203. Li20 (bk) -0.16843 B203 .Na20 (b) -0.28237 B203. K20 (b) -0.27890 Na2 0 .Li20 (b k) 0.20691 Na2O. K2O (b) 0.58773 Na2O. Ca0 (b) 0.19254 K20. Li20 (b) 0.24924 K20. Mg0 (b) 0.59449 K20. Ca0 (b) 0.29628 MgO. Ca0 (b) -0.17394 Al 2 O 3 .Na 2 O. CaO (bikm) 0.033620 As an exemplary embodiment, a high-strength borosilicate glass according to the invention is compared with a borosilicate glass bearing the designation Borofloat 33. The composition of these glasses is as follows: Glass Si02 B203 A1203 K20 Na20 Borofloat 33 Composition 81 12.5 2.5 0.5 3.5 (percent by weight Glass 1 Composition 79.5 16.5 1 0 3 (percent by weight) First, with converted composition of 81.76 mol% of SiO 2, 14.64 mol% of B 2 O 3, 0.61 mol% of Al 2 O 3, 2.99 mol% of Na 2 O, and the coefficient of expansion which is calculated from according to equation (17) above and which is 3.51 ppm / K at 210 ° C, the glass according to the invention (designated as "Glass 1") meets the requirement for glasses according to the invention to be less than 3.6 ppm / K. The weighted crosslinking number is 2.911. On the other hand, the melting point is below 1600 ° C. and is 1535 ° C. according to the formula (22 ).
[0031] For comparison, with the converted composition of 83.53 mol%. SiO2, 11.12% mol. of B203, 1.52 mol%. of A1203, 3.50 mol%. Na 2 O and 0.33 mol%. of K20, and the coefficient of expansion calculated from it according to equation (17) above and which is 3.69 ppm / K at 210 ° C, Borofloat 33 does not respond to condition for the glasses according to the invention to be less than 3.6 ppm / K. In addition, the weighted crosslinking index of Borofloat 33 at the value of 2.893 and is therefore less than the minimum value of 2.9 required according to the invention. The melting temperature according to formula (22) is 1 553 ° C.
[0032] Since the melting temperature of the glass according to the invention must not increase appreciably and must rather decrease with respect to Borofloat 33, the improvement of the invention lies in the fact that the melting temperature must remain, according to the equation (22), below 1 570 ° C, preferably below 1 560 ° C, particularly preferably below 1 550 ° C and most preferably below 1 540 ° C. In experiments, we found for the charge "Crack Initiation Load" (CIL), which according to Trevor Wilantewicz, Crack Initiation Behavior of Optical Glasses from Vickers Indentation, Dissertation, Alfred University, Alfred, NY, USA, 2005, is in coarse correlation with the value c / a, a value of 12.3 +/- 1N for glass 1, compared to 6.9 +/- 0.4N for Borofloat 33. CIL is the force with which on average 2 cracks form from the angles of a Vickers fingerprint. In order to determine the CIL, several Vickers impressions are produced with different impression forces and the cracks forming at the angles are counted. The average number of cracks is plotted against the test force and a discontinuous adjustment function is passed through the measurement points.
[0033] For this adjustment function, 0 is defined as the smallest value and 4 as the largest value. The inflection point of the curve is the CIL. The maximum force was 20 N. During the measurements, the samples are in a test chamber into which a constant stream of dry nitrogen is sent.
[0034] The glass compositions selected with the method according to the invention are distributed over the range of general compositions with 70 to 86% by weight of SiO 2, since the components influence each other in their effects on the number of stress conditions and on the coefficient of expansion.
[0035] The table below indicates some preferred composition ranges for glasses according to the invention. Range 1 Range 2 Range 3 Range 4 Range 5 Range 6 Weight percent SiO 2 79 - 80 81.5 - 83.5 85 - 86 80-82 75 - 77 71.2 - 73.2 B203 16 - 17 11.5 - 13 11.5 - 13 14 - 16 19 -21 23.8 -25.8 A1203 0.5-1.5 2-3 0 0.5-1.5 0.8-2 0.5-1, Li 2 O 0 0 0 0 0.25-0.75 Na 2 O 4 2-4 1-3 2 - 4 2-3 0.25-0.75 1 (20 0 0.1 - 1 0 0 0, 05-0.2 0.5-1.5 MgO 0 0 0 0 0 0 CaO 0 0 0 0 0 0 BaO 0 0 0 0 0 0 With regard to the network formers Si02 and B203, it is furthermore advantageous, in accordance with An improvement of the invention, that their total content, i.e., the sum of the SiO 2 and B 2 O 3 contents, is in the range of 95.5% by weight to 97.5% by weight. weight, preferably in the range of 95.8% by weight to 97.2% by weight, particularly preferably up to 97.1% by weight.Indicated in percent molar, it is advantageous to have a total content in the range of 95.5 mol% to 97.5 mol%, preferably in the range of 95.7 mol% to 97.2% mol., particularly preferably up to 97.1 mol%. A high fraction of these network formers is advantageous for low fragility. On the other hand, the indicated upper limits are advantageous for obtaining a high hardness, since the residual content of other components increases correspondingly. These other components can be incorporated in the interstices of the glassy network and thus increase the hardness of the glass. In other words, the ranges indicated for the total contents of network formers are advantageous in order to obtain both low brittleness and high hardness. Hereinafter, some exemplary embodiments which correspond to the parameters according to the invention n> 2.9 and a (210 ° C.) <3.6 '10-6 K-1 and are within the ranges indicated in FIG. -above. The glass 1 is an exemplary embodiment for the beach 1, the glass 2 is an embodiment for the beach 2, and so on, and the glass 6 is an embodiment for the beach 6. Glass 1 Glass 2 Glass 3 Glass 4 Glass 5 Glass 6 Weight percent SiO 2 79.5 82.15 85.8 81 76 72 B203 16.5 12.1 12.1 15 20 25 A1203 1 2.4 0 1 1.3 1 Li20 0 0 0 0 0 0.5 Na20 3 2.95 2.1 3 2.6 0.5 1 (20 0 0.4 0 0 0.1 1 MgO 0 0 0 0 0 0 CaO 0 0 0 0 0 0 BaO 0 0 0 0 0 0 Molar percentage SiO 2 81.76 84.58 87.3 83.13 78.67 74.77 B203 14.64 10.75 10.63 13.29 17.87 22.41 A1203 0, 61 1.46 0.6 0.79 0.61 Li20 0 1.04 Na20 2.99 2.94 2.07 2.98 2.61 0.5 K20 0.26 0.07 0.66 MgO 0 0 CaO 0 0 BaO 0 0 CTE at 210 ° C according to 3,51 3,44 3,073 3,47 3,486 3.31 equ. (17) [pm / K] Melting temperature 1535 1576 1572 1541 1547 1588 according to equation (22 ) [° C] Crosslinking index 2.911 2.905 2.940 2.917 2.908 2.911 effective The glass 1 of the table is identical to the glass 1 of the embodiment described above. below are examples of comparison: Schott Glass Glass Glass Glass Glass Glass Verr Verrel Boro33 7 8 9 10 11 12 e 4 13 Percent by weight SiO 2 81 80.9 81.2 80.6 79.3 66 79 79, 8 78.6 B203 12.5 12.8 12.5 13.2 13.6 25 10 13.4 10.6 A1203 2.5 2.2 2.2 2 2.5 5 4 2.2 4.3 Li20 0 0 0 0 0 0,6 0 0 0 Na20 3,5 4,1 4,1 4 3,9 3,2 5 4,3 4,7 K20 0,5 0 0,05 0,2 0,7 0 1 0.1 0.8 MgO 0 0 0 0 0 0 0 0 0.2 CaO 0 0 0 0 0 0 1 0 1.3 BaO 0 0 0 0 0 0 0 0 0 Percent mol. Si02 83.53 83.21 83.50 82.9 81.97 69.46 81.83 82.1 81.40 4 9 B203 11.12 11.36 11.09 11.7 12.13 22.71 8 , 94 11.9 9.47 2 1 A1203 1.52 1.33 1.33 1.21 1.52 3.10 2.44 1.34 2.62 Li2O 0.00 0.00 0.00 0, 0.00 0.00 1.27 0.00 0.00 0.00 Na2 O 3.50 4.09 4.09 3.99 3.91 3.26 5.02 4.29 4.72 K20 0.33 0, 00 0.03 0.13 0.46 0.00 0.66 0.07 0.53 MgO 0.00 0.00 0.00 0.00 0.00 0.00 0.00 0.31 CaO 0,00 0,00 0,00 0,00 0,00 0,00 1,11 0,00 1,44 BaO 0,00 0,00 0,00 0,00 0,00 0,00 0,00 0.00 0.00 CTE at 210 ° C 3.69 3.80 3.80 3.91 3.83 4.06 4.49 3.91 4.37 according to equ. Gl. (17) [pm / KI Temp. of 1553 1542 1532 1525 1597 1523 1527 melting according to equ. (22) [° C1 Index of 2,893 2,891 2,891 2,89 2,883 2,851 2,850 2,88 2,851 crosslinking 1 6 effective The first glass cited among these comparative examples is Borofloat 33 already described above. The glasses of the comparison examples also show a wide variability in the concentrations of the various components. However, in the case of the comparison examples, they have a joint action such that, at the same time, the constraint conditions per atom are lower and the coefficient of expansion is greater than for the glasses according to the invention. .
[0036] The glasses according to the invention are particularly suitable for hot forming by floating process. Therefore, according to an improvement of the invention, it is provided that the method comprises forming a plate-shaped glass member from molten glass, preferably by floating. In general, the glasses according to the invention are preferably converted into glass elements in the form of plates or panes for the most diverse applications.
[0037] Especially for plate-shaped glass elements, the strength of the glass is of particular importance to prevent breakage or bursting in the presence of mechanical stresses. This also applies to fire-resistant glazing where large temperature differences in the event of a fire must not cause stress resulting in failure. The intrinsic resistance of the glasses according to the invention is now so great and the brittleness so low that in many cases it is not necessary to carry out thermal or chemical quenching. Therefore, according to an improvement of the invention, the glass according to the invention is implemented to form a glass element which is not tempered. Some residual stresses, due to manufacture, are not excluded, but preferably the compressive stress at the surface is less than 10 MPa, or the surface is free of compressive stresses. In comparison, thermally toughened glasses have compressive stresses of more than 100 MPa. Another preferred embodiment is tubular glass elements, for example for glass pipes. Apart from chemical resistance, resistance also plays an important role in ensuring the safe passage of aggressive fluids. On the other hand, the glasses are also suitable for household appliances, such as cooking vessels. Other particularly suitable uses are mentioned above in the part relating to the subject of the invention.
权利要求:
Claims (13)
[0001]
REVENDICATIONS1. High strength alkaline borosilicate glass, comprising the following components: SiO 2 70 - 86 wt.% A1203 0 - 5 wt.% B203 9.0 - 25 wt.% Na2 O 0.5 - 5.0 wt.% K20 0 - 1 , 0% by weight Li 0 0 - 1.0% by weight, as well as 0 - 5.0% by weight of other constituents, where the proportions of the components are chosen such that the weighted crosslinking index, that is the number n average of the stress conditions per atom, defined by c (SiO2) -3 + c (A / 203) -5 + c (/ 3203) -5 + Ic (M'20) .3 + Ic (M-10). 2 has a value greater than 2.9, preferably greater than 2.91, particularly preferably greater than 2.92, and most preferably greater than 2.93, where NA denotes the number of Avogadro and c (SiO 2). , c (Al 2 O 3) and c (B 2 O 3) the molar concentrations of SiO 2, Al 2 O 3 and B 2 O 3, c (1 4120) denote the molar concentrations of the alkali oxides 1 4'20 contained and c (MO) the molar fractions of the alkaline oxides -terrous content, and where the N / NA ratio is finished with N - c (SiO
[0002]
2) - 9 K (Al-o) e (Al-0) 14 + c (Al 20
[0003]
3) - 2 - 4 + 5 - K (Si - 0) e (Si - 0) 14 ' c (1 / R0) +1 c (1/0) - c (Al 2 O) - 2 - 4 + 5 - K (B - ed (B - 0) 14 3 K (Si - O), e (Si - O) 14 c (B 2 O 3) + c (Al 3 O 3) - c (11/1; 0) - c ( 11/1 '0) .2, 33 K (B -O) ed (B - 0) / 3 + - K (Si - 0), e (Si - O) / 4 + I 41/10) 2 ed ( M '-O) e - 0) / 4 +1 c (11/1' 0) 2 e (IVI O) 12 e (Si - 0) 1 where K (M - O), M = Si, Al, B are the covalent degrees of the respective M-O bonds of the components 5iO 2, Al 2 O 3, B 2 O 3, namely: a degree of covalency of 0.5527 for 5iO 2, a degree of covalence of 0.6126 for B 2 O 3, and a degree of covalently 0.4329 for Al 2 O 3, and where the ed (M-0) are the cation-dependent dissociation energies of the components 5102, A1203, B203 and are defined by: 1864 kJ / mol for 5i02, 1572 , 5 kJ / mol for B203, and 1537 kJ / mol for A1203. 2. Alkali borosilicate glass according to the preceding claim, characterized in that the glass has a coefficient of linear thermal expansion of less than 3.6 ppm / K, at a temperature of 210 ° C. 3. Alkali borosilicate glass according to the preceding claim, characterized in that the components of the glass are chosen such that the value of the coefficient of linear thermal expansion, which is determined according to the equation No. 13 (210 ° C) = 130 ± 13j - Cj + 13j2 - Cj2 I13jk - Cj - Ck j = 1 k = j + 1 is less than 3.6 '10-6 K-1, at a temperature of 210 ° C, where Cj, Ck are the molar concentrations ( in mole percent) of the respective components of the glass composition, and where the coefficients Bo, Bi, Bi2, Bik are applied: Coefficient Value Portion of axis (130) 1.7672 Na2O (Bi) 0.4545 Na2O (13i2) -0.001198 Ca0 (13i) 0.1682 Al2O3 (13i) -0.0641 Al2O3 (Bi2) 0.006473 K20 (13i) 0.5320 K20 (Bi2) -0.001710 MgO (Bi) 0.0499 B203 (Bi) 0.0465 Li20 (13i) 0.1896 Li2 O (13i2) 0.003242 Sr ) (13i) 0.1717 BaO (13i) 0.3077 ZrO2 (13i) -0.0591 TiO2 (13i) -0.0138 ZnO (13i) 0.0102 PbO (13i) 0.1345 F (13i) 0.1305 Na2O * Ca0 (131) -0.002579 Na2O * B203 (4) ) -0.005640 Na2O * Li2O (13ik) 0. 018869 CaO * Mg0 (13ik) 0.002627 Ca0 * B203 (13I1) -0.002682 CaO * Ba0 (13I1) -0.011958 K20 * B203 (4) -0.012682.
[0004]
4. An alkaline borosilicate glass according to one of the preceding claims, characterized in that the composition is selected from one of the following composition ranges: Range 1 Range 2 Range 3 Range 4 Range 5 Range 6 Weight percent SiO 2 79 - 80 81.5 - 83.5 85 - 86 80-82 75 - 77 71.2 - 73.2 B203 16 - 17 11.5 - 13 11.5 - 13 14 - 16 19 -21 23.8 -25 , 8 A1203 0.5 - 1.5 2-3 0 0.5 - 1.5 0.8-2 0.5 - 1.5 Li20 0 0 0 0 0 0.25 - 0.75 Na2O 2 - 4 2 - 4 1-3 2 - 4 2-3 0.25 - 0.75 1 (20 0 0.1 - 1 0 0 0.05 - 0.2 0.5 - 1.5 MgO 0 0 0 0 0 0 CaO 0 0 0 0 0 0 BaO 0 0 0 0 0 0 10 15 25 30
[0005]
Alkaline borosilicate glass according to one of the preceding claims, characterized in that the sum of the SiO 2 and B 2 O 3 contents is in the range of 95.5% by weight to 97.5% by weight, preferably in the range from a range of 95.8% by weight to 97.2% by weight, and particularly preferably up to 97.1% by weight, or the sum of the SiO 2 and B 2 O 3 contents is in the range of 95, 5 mol% to 97.5 mol%, preferably in the range of 95.7 mol% to 97.2 mol%, and particularly preferably up to 97.1 mol%.
[0006]
6. A glass element comprising an alkaline borosilicate glass according to one of the preceding claims, preferably in the form of a plate-shaped glass element or tube.
[0007]
7. Glass element according to the preceding claim, characterized in that it has a compression stress on the surface which is less than 10 MPa.
[0008]
A method of manufacturing a glass element, wherein a composition of a borosilicate glass is selected, in a compositional range with the following components, in weight percent: SiO 2 75 - 86 wt% Al 2 O 3 0 - 5% by weight B203 9.0 - 25% by weight Na2O 0.5 - 5.0% by weight K20 0 - 1.0% by weight Li2O 0 - 1.0% by weight, as well as 0 - 5.0 other components, which meets the requirement that the weighted crosslinking index be the average number of stress conditions per atom, defined by n = c (SiO 2) - 3 + c (A / 203) - 5 + c (/ 3203) - 5 + c (M120). 3 + »'O). 2presents a value greater than 2.9, preferably greater than 2.91, particularly preferably greater than 2.92, and most preferably greater than 2.93, where NA denotes the number of Avogadro and c (SiO2), c (Al 2 O 3) and c (B 2 O 3) the molar concentrations of SiO 2, Al 2 O 3 and B 2 O 3, c (1 4120) denote the molar concentrations of the alkali metal oxides 1 4'20 contained and c (1 4'0) the molar fractions contained alkaline earth oxides, and wherein the N / NA ratio is defined as N = c (SiO 2) - 9 - K (Al - o) e (Al - O) 14 + c (Al 2 O 3) - 2 - 4 + 5 - - K (Si - 0) e (Si - 0) 1 4 ' 1 c (1 I 1; 0) +1 4 I' 0) - c (Al 2 3) - 2 - 4 + 5 - K (B - ed (B - 0) 1 4 K (Si - O), e (Si - O) 1 4 c (B 2 O 3) + c (A / 203) - c (71/1; O) -: c (11 / 1'0) -2 - 3 + 3 - - K (B -O) ed (B-O) 13 -K (Si-O), e (Si-O) 14 + 141; O) 2 ed (M '-' 9) e (SI - 0) 1 4 +1 4 1 1 '0) 2 ed (IV e (SI - 0) 1 4 where K (M - O), M = Si, Al , B, are the covalent degrees of the respective M-O bonds of the components 5iO 2, Al 2 O 3, B 2 O 3, at its see: a degree of covalency of 0.5527 for 5iO2, a degree of covalence of 0.6126 for B203, and a degree of covalency of 0.4329 for A1203, and where ed (M-0) are the dissociation energies 5O 2, Al 2 O 3, B 2 O 3 and are defined as: 1864 kJ / mol for 5iO 2, 1572.5 kJ / mol for B 2 O 3, and 1537 kJ / mol for Al 2 O 3. and melting a glass having the determined glass composition, and forming a glass member from the molten glass.
[0009]
9. Method according to the preceding claim, characterized in that the glass composition is chosen so that the glass has a coefficient of linear thermal expansion below 3.6 ppm / K at a temperature of 210 ° C.
[0010]
10. Method according to the preceding claim, characterized in that the components of the glass are chosen such that the value of the coefficient of linear thermal expansion, which is determined according to the equation n "ct (210 ° C) = po +1 13, -c, + E3,2-C, 2 + Ejk -c, - Ck j = 1 k = j + 1 is less than 3,6 '10-6 K-1, at a temperature of 210 ° C, where Ci , Ck are the molar concentrations (in mole percent) of the respective components of the glass composition, and where the coefficients Bo, Bi, Bi2, Bik are applied: Coefficient Value Portion of axis (Bo) 1.7672 Na 2 O (Bi) 0.4545 Na2 O (13i) -0.001198 Ca (13i) 0.1682 Al2O3 (13i) -0.0641 Al2O3 (Bi2) 0.006473 K20 (13i) 0.5320 K20 (Bi2) -0.001710 MgO (Bi) 0.0499 B203 (Bi) 0.0465 Li2O (Bi) 0.1896 Li20 (13i2) 0.003242 Sr () (Bi) 0.1717 BaO (Bi) 0.3077 ZrO2 (B) -0.0591 TiO2 (13i) -0.0138 ZnO (Bi) 0.0102 Pb0 (Bi) 0.1345 F (Bi) 0.1305 Na2O * Ca0 (bg) -0.002579 Na20 * B203 (13ik) -0.005640 Na2O * Li2O (Bik) 0.018869 CaO * MgO (14) 0.002627CaO * B2 03 (4) -0.002682 CaO * Ba0 (13jk) -0.011958 K20 * B203 (4) -0.012682.
[0011]
11. Method according to one of claims 8 to 10, characterized in that the composition is chosen from one of the following composition ranges: Range 1 Range 2 Range 3 Range 4 Range 5 Range 6 Weight percent SiO2 79 - 80 81.5 - 83.5 85 - 86 80-82 75 - 77 71.2 - 73.2 B203 16- 17 11.5- 13 11.5- 13 14- 16 19- 21 23.8-25, 8 A1203 0.5 - 1.5 2 - 3 0 0.5 - 1.5 0.8 - 2 0.5 - 1.5 Li20 0 0 0 0 0 0.25 - 0.75 Na 2 O 2 - 4 2 - 4 1 - 3 2 - 4 2 - 3 0.25 - 0.75 K20 0 0.1 - 1 0 0 0.05 - 0.2 0.5 - 1.5 MgO 0 0 0 0 0 0 CaO 0 0 0 0 0 0 BaO 0 0 0 0 0 0
[0012]
Method according to one of the preceding claims, characterized in that the forming of a glass element includes the forming of a plate-shaped glass element by floating from the molten glass.
[0013]
13. Use of the glass according to one of claims 1 to 5 or the glass element according to one of claims 6 or 7, as - fire-resistant glazing - structural element with high resistance to static loads in the field of building, for example as a facade element, - glazing for protection against heat, in particular for cooking appliances or cooking ovens or as glass for pyrolysis ovens, 20 20- induction cooking surface , - glass pipe element, - plate for glazing without putty, - anti-ballistic glazing.
类似技术:
公开号 | 公开日 | 专利标题
FR3030488A1|2016-06-24|BOROSILICATE GLASS WITH LOW FRAGILITY AND HIGH INTRINSIC RESISTANCE, MANUFACTURE AND USE THEREOF
JP6778290B2|2020-10-28|High-strength glass-ceramic with lithium disilicate and β-spodumene structure
JP6942210B2|2021-09-29|High-strength glass-ceramic with petalite and lithium silicate structures
Hench et al.1978|Physical chemistry of glass surfaces
Vogel2012|Glass chemistry
US4455160A|1984-06-19|Transparent glass-ceramics especially suitable for use as stove windows
Ropp2013|Inorganic polymeric glasses
JP2009517319A|2009-04-30|Crystal-free glass frit composition and frit produced therefrom for microreactor devices
TW201925129A|2019-07-01|Black lithium silicate glass ceramics
Bayya et al.1997|BaO Ga2O3 GeO2 glasses with enhanced properties
Fernández-Navarro et al.2013|What is glass
Souza et al.2011|Liquid–Liquid Phase Separation in Photo‐Thermo‐Refractive Glass
Karasu et al.2000|The chemical durability of SrO–MgO–ZrO2–SiO2 glasses in strongly alkaline environments
Krause2018|Glasses
FR2939427A1|2010-06-11|TRANSPARENT AND LOW-DENSE GLASS-CERAMIC AND USE THEREOF
Carter et al.2013|Glass and glass-ceramics
Kilinc2016|Mechanical and structural properties of soda lime silica glasses as a function of composition.
JP7027594B2|2022-03-01|High-strength glass-ceramic with petalite and lithium silicate structures
Conradt2021|Glass Production: An Overview
Basu et al.2019|Glass processing and properties
JPWO2019150654A1|2020-11-26|Chemical strengthening glass
Browder et al.2017|Physical Properties of Glass Infrared Optical Materials
Carter et al.2007|Glass and glass-ceramics
Delaizir2007|Nanoporous glass-ceramics transparent in infrared range to be used as optical sensor: Mechanical and viscoelastic properties of the TAS | glass
Hülsenberg et al.2008|Silicate glasses: a class of amorphous materials
同族专利:
公开号 | 公开日
US10442723B2|2019-10-15|
JP2016147796A|2016-08-18|
JP6725984B2|2020-07-22|
US20160176751A1|2016-06-23|
CN105712623A|2016-06-29|
DE102014119594A1|2016-06-23|
DE102014119594B9|2020-06-18|
CN105712623B|2020-09-29|
DE102014119594B4|2019-02-07|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题

DE588643C|1915-06-24|1933-11-21|Corning Glass Works|Process for the production of a heat-resistant glass|
GB207911A|1922-09-18|1923-12-13|Marmet Baby Carriage Syndicate|Improvements relating to perambulators and the like|
NL6411555A|1963-12-04|1965-06-07|
DE2413552B2|1974-03-21|1976-09-02|Jenaer Glaswerk Schott & Gen., 6500 Mainz|FIRE-PROOF GLASS PANELS|
FR2389582B1|1977-05-04|1980-01-18|Saint Gobain|
DE2756555C3|1977-12-19|1982-12-02|Schott Glaswerke, 6500 Mainz|Thermally toughenable glasses with high thermal shock resistance and thermal expansion coefficients in the temperature range from 20 to 300 ° C from 33.9 to 53.2 times 10 - 7 / ° C based on SiO 2 -B 2 O ; 3 -Al 2 O 3 -Na 2 O|
GB2079119A|1980-06-17|1982-01-13|Bfg Glassgroup|Vitreous cooking hob|
JPS6124344B2|1981-03-30|1986-06-10|Toshiba Glass Kk|
JPH03337B2|1982-02-23|1991-01-07|Asahi Glass Co Ltd|
JPS6124344A|1984-07-13|1986-02-03|Hitachi Ltd|Pos system|
SU1284959A1|1985-04-02|1987-01-23|Gnii Stekla|Heat-resistant glass|
DE3722130C2|1987-07-02|1989-12-28|Schott Glaswerke, 6500 Mainz, De|
JPH0561214B2|1987-10-05|1993-09-03|Nippon Sheet Glass Co Ltd|
DE4012288C1|1990-04-17|1991-07-18|Schott Glaswerke, 6500 Mainz, De|
FR2692883B1|1992-06-25|1994-12-02|Saint Gobain Vitrage Int|Thermally stable and chemically resistant glasses.|
DE4230607C1|1992-09-12|1994-01-05|Schott Glaswerke|Chemically and thermally highly durable, can be fused with tungsten borosilicate glass and its use|
DE4325656C2|1993-07-30|1996-08-29|Schott Glaswerke|Use of a glass body for producing a tempered glass body suitable as a fire protection safety glass on a conventional air pretensioning system|
DE4428235C1|1994-08-10|1995-11-02|Jenaer Glaswerk Gmbh|Colored borosilicate glass and its use|
DE4430710C1|1994-08-30|1996-05-02|Jenaer Glaswerk Gmbh|Low boric acid borosilicate glass and its use|
FR2727399B1|1994-10-13|1997-01-31|Saint Gobain Vitrage|SILICO-SODO-CALCIUM GLASS COMPOSITIONS AND THEIR APPLICATIONS|
DK42495A|1995-04-07|1996-10-08|Electrolux Ab|Surface for induction cooker|
DE19515608C1|1995-04-28|1996-08-08|Ilmenau Tech Glas|Borosilicate glass with linear thermal expansion|
DE19643870C2|1996-10-30|1999-09-23|Schott Glas|Use of a glass body to produce a chemically toughened glass body|
DE19913227C1|1999-03-23|2000-07-27|Schott Glas|Borosilicate glass of specified composition is used for production of thermal cycling resistant beverage containers, especially coffee machine jugs, tea-pots and baby milk bottles|
DE10122718C2|2001-05-10|2003-04-17|Schott Glas|Process for producing a layer of scattered light on a transparent hotplate and its use|
JP4310948B2|2001-09-06|2009-08-12|鳴海製陶株式会社|Top plate for cooker|
DE10150884A1|2001-10-16|2003-05-08|Schott Glas|Alkali borosilicate glass used in the production of flat glass comprises oxides of silicon, boron, aluminum, sodium and potassium, and optionally calcium|
JP3900939B2|2002-01-22|2007-04-04|鳴海製陶株式会社|Cooker top plate|
WO2003098115A1|2002-05-16|2003-11-27|Nippon Electric Glass Co., Ltd.|Cooking top plate|
DE10239180A1|2002-08-21|2004-03-04|BSH Bosch und Siemens Hausgeräte GmbH|Cooking chamber door of a cooking oven with pyrolysis function|
DE10243500A1|2002-09-19|2004-04-01|Schott Glas|Cooking surface for hobs, consists of a transparent non-colored glass-ceramic plate or glass plate with an IR-permeable layer made from a temperature-stable inorganic enamel paint containing a glass flow and inorganic pigments|
DE10355160B4|2003-11-26|2008-04-03|Schott Ag|Coated glass ceramic plate, method for its production and hob with such a glass ceramic plate|
DE102005059744A1|2005-12-14|2007-06-28|Man Roland Druckmaschinen Ag|Extraction arrangement for a boom of a sheet-fed press|
JP2008145637A|2006-12-08|2008-06-26|Kyocera Mita Corp|Image forming apparatus|
TW200835661A|2007-02-27|2008-09-01|United Oriental Glass Ind Co Ltd|Borosilicate glass composition|
CN101274816B|2007-03-29|2011-10-19|东联光讯玻璃股份有限公司|Borosilicate glass constituent|
DE102009031972B4|2009-07-02|2013-01-03|Schott Ag|Photovoltaic module and use of a glass for a photovoltaic module|
CN101891381B|2010-07-28|2011-11-16|济南力诺玻璃制品有限公司|High borosilicate glass for storing frozen biological products and preparation method thereof|
FR2974700B1|2011-04-29|2013-04-12|Eurokera|INDUCTION COOKING DEVICE|
JP2014093437A|2012-11-05|2014-05-19|Ricoh Co Ltd|Laser pumped laser device and process of manufacturing the same|KR20170088397A|2014-11-26|2017-08-01|코닝 인코포레이티드|Strengthened glass, glass-ceramic and ceramic articles and methods of making the same through pressurized ion exchange|
DE102017102485A1|2017-02-08|2018-08-09|Schott Ag|Glasses with improved hydrolytic and alkali resistance|
DE102017102482B4|2017-02-08|2019-11-21|Schott Ag|Glasses with improved ion exchangeability and thermal expansion|
US11152294B2|2018-04-09|2021-10-19|Corning Incorporated|Hermetic metallized via with improved reliability|
DE102018112070A1|2018-05-18|2019-11-21|Schott Ag|Flat glass, process for its production and its use|
DE102018112069A1|2018-05-18|2019-11-21|Schott Ag|Use of a flat glass in electronic components|
DE102018116464A1|2018-07-06|2020-01-09|Schott Ag|Chemically toughened, corrosion-resistant glasses|
DE102019117498A1|2018-07-06|2020-01-09|Schott Ag|Glasses with improved ion interchangeability|
DE102018116460A1|2018-07-06|2020-01-09|Schott Ag|Highly resistant and chemically toughened glasses|
DE102018116483A1|2018-07-06|2020-01-09|Schott Ag|Chemically toughened glasses with high chemical resistance and crack resistance|
US20210322283A1|2018-09-04|2021-10-21|3M Innovative Properties Company|Glazing composition for a dental zirconia article, process of sintering and kit of parts|
DE102018133413A1|2018-12-21|2020-06-25|Schott Ag|Chemically resistant, boron and alkali free glasses|
DE102019135597A1|2019-12-20|2021-06-24|Schott Ag|Thermally toughenable borosilicate glasses|
JP2021176817A|2020-05-08|2021-11-11|ショット アクチエンゲゼルシャフトSchott AG|Strengthening due to use of gradient material|
法律状态:
2016-12-22| PLFP| Fee payment|Year of fee payment: 2 |
2017-12-21| PLFP| Fee payment|Year of fee payment: 3 |
2019-12-19| PLFP| Fee payment|Year of fee payment: 5 |
2020-12-23| PLFP| Fee payment|Year of fee payment: 6 |
2021-10-29| PLSC| Publication of the preliminary search report|Effective date: 20211029 |
2021-12-24| PLFP| Fee payment|Year of fee payment: 7 |
优先权:
申请号 | 申请日 | 专利标题
DE102014119594.9A|DE102014119594B9|2014-12-23|2014-12-23|Low brittleness and high intrinsic strength borosilicate glass, its manufacture and use|
[返回顶部]