专利摘要:
A method of modifying an open porosity cellular polymeric foam, preferably polyurethane, comprising the steps of: a) supplying an open porosity cellular polymer foam (a); b) said cellular polymer foam is brought into contact with at least one compound (b) chosen from compounds comprising at least one catechol unit, and preferably from catecholamines, to obtain a cellular polymer foam comprising on its surface an intermediate phase formed from said compound having at least one catechol pattern. This foam can be used as a catalyst support or as a filter.
公开号:FR3024147A1
申请号:FR1457055
申请日:2014-07-22
公开日:2016-01-29
发明作者:David Edouard;Vincent Ritleng;Loic Jierry;Dalencon Nguyet Trang Thanh Chau
申请人:Centre National de la Recherche Scientifique CNRS;Universite Claude Bernard Lyon 1 UCBL;Universite de Strasbourg;
IPC主号:
专利说明:

[0001] FIELD OF THE INVENTION The invention relates to the field of porous solid materials, more particularly cellular polymer foams. It relates to a method for surface modification of elastomeric cellular foams, in particular foams with open porosity, for use as a catalyst support or as a selective filter. STATE OF THE ART Many catalysts are known whose catalytic phase is present in a porous solid material, and more particularly adsorbed on the surface of a ceramic or metallic cellular foam. For example, the most widely used method of producing ceramic foams is the impregnation of a polymeric foam, most often a polyurethane or polyester foam, cut to the desired geometry, by a suspension of ceramic particles in a aqueous or organic solvent. The excess suspension is removed from the polymer foam by repeated application of compression or centrifugation, in order to keep only a thin layer of suspension on the strands of the polymer. After one or more impregnations of the polymeric foam, the latter is dried so as to evacuate the solvent while maintaining the mechanical integrity of the deposited ceramic powder layer. The foam is then sintered to obtain an inorganic foam which can be used as a catalyst support. This rather complex manufacturing process generates a fairly high manufacturing cost. One of the advantages of ceramic foams is their chemical and thermal resistance. However, excellent heat resistance is not always required. In addition, ceramic foams have the disadvantage of concealing microcracks and other microstructural defects considerably lowering their mechanical properties. In addition, in many cases, the recovery of the metal active phase (catalyst) requires many chemical treatments. An object of the present invention is to provide novel catalyst supports which are an alternative to metal or ceramic foam catalyst supports currently used in the chemical, pharmaceutical and / or cosmetic industry in environments that do not require thermal resistance. high, which are easy to prepare, and that with a low manufacturing cost, and which have similar or advantageous structural characteristics.
[0002] Another object of the present invention is to provide novel catalysts for heterogeneous and / or homogeneous catalysis supported, with a low pressure drop and having a large specific surface area, while having a very good chemical inertness, and which are available in all types of geometric shapes (square, planar, cylindrical, etc.) and flexible from a mechanical point of view. Objects of the invention According to the invention the problem is solved by chemically modifying the surface of a known cellular material, namely a cellular foam (in particular an elastomer) with open porosity. Cellular polymeric foams (also called "cellular foam") are well known and are commercially available for many applications. When made of closed cells, they exhibit excellent mechanical strength and are used as cushioning foam, packaging foam, or in mechanical engineering. At the same time these closed cells trap air and thus give the foams excellent thermal insulation properties, which are exploited in the building sector. Polymeric foams (in particular elastomers) with open porosity (called "open cell polymer polymer") are also known, in which only the edges of the cells consist of solid polymer. These include polyurethane foams. They are used as filters, especially in aquariums. However, these foams can not be used as a catalyst support because of the poor adhesion of the catalysts (or their precursor compounds) to the surface of this polymer.
[0003] Their use as a catalyst support encounters the difficulty of depositing a catalytically active phase or an active phase precursor phase. Indeed, the surface of the bridges (edges) polymers is smooth, devoid of microporosity, and does not have sufficient adhesion to deposit the precursor molecules or active phases usually used in homogeneous or heterogeneous catalysis. For this reason, open-pored cellular polymeric foams have hardly been considered as candidates for the manufacture of catalyst supports. The inventors have found a suitable surface treatment which prepares cellular (in particular elastomer) cellular foams, and in particular those with open porosity, to receive a catalytically active phase deposition (here called "active phase") or a phase of active phase precursor. A first object of the present invention is a method of modifying an open porosity cellular polymeric foam, preferably polyurethane, comprising the following steps: a) supplying an open porosity cellular polymer foam (a); b) said cellular polymer foam is brought into contact with at least one compound (b) chosen from compounds comprising at least one catechol unit, and preferably from catecholamines, to obtain a cellular polymeric foam comprising on its surface a phase intermediate formed from said compound having at least one catechol pattern. Said cellular polymeric foam is advantageously a polyurethane foam. In one embodiment, the step of contacting said cellular polymeric foam (a) and the compound (b) is performed by immersing said cellular polymeric foam (a) in an aqueous solution of compound (b), or by impregnating an aqueous solution of compound (b) on said cellular polymeric foam (a), or by partially or completely spraying an aqueous solution of compound (b) onto said cellular polymeric foam (a).
[0004] Advantageously, said cellular polymer foam (a) comprises cells of average size between 500 μm and 5000 μm, preferably between 2000 μm and 4500 μm, and even more preferably between 2500 μm and 4500 μm; these values are chosen for use of the foams as a catalyst support or as a selective filter.
[0005] Compound (b) is advantageously selected from catecholamines, and is more particularly 4- (2-aminoethyl) benzene-1,2-diol, or a derivative thereof. The method according to the invention may further comprise a step c) of functionalizing said cellular polymer foam by depositing a phase of at least one catalytically active material (c) or catalytically active phase precursor, said at least one material (c) being selected from the group consisting of: metal complexes comprising at least one group capable of forming covalent bonds with the catechol structural element, for example a trialkoxysilane group, an amine group or a thiol group, and more particularly coordination compounds or organometallic molecules of transition metals. The metallic nanoparticles, preferably the metal nanoparticles chosen from those of Ag, Fe, Co, Ni, Ru, Rh, Pd, Ir, Pt, Au, Ce, or those of the mixed oxides associated with these elements, such as Fe 2 O 3, NiO 2, Ni 2 O 3, CeO 2, as well as among those of other oxides, such as TiO 2, ZnO, WO 3, SnO 2, or any possible combinations of these nanoparticles. According to one embodiment, the functionalization step is carried out at a temperature of between 5 and 80 ° C., preferably between 15 and 60 ° C., and even more preferably between 15 and 50 ° C.
[0006] Said metal nanoparticles have an average particle size of between 0.5 and 30 nm, preferably between 0.5 and 20 nm, and even more preferably between 0.5 and 15 nm. Said catalytically active phase or catalytically active phase precursor can be deposited by at least one of the following techniques: by impregnation, by aerosol, or by droplets; - by chemical vapor deposition; - by capillary impregnation.
[0007] Another object of the invention is an open porosity functionalized cellular polymer foam obtainable by the process according to the invention. Yet another object of the invention is the use of an open porosity cellular polymer foam obtainable by the process according to the invention as a catalyst support or as a filter. Yet another object of the invention is the use of an open porosity functionalized cellular polymer foam obtainable by the process according to the invention as a catalyst, and more particularly as a supported homogeneous catalyst and or heterogeneous, or as a selective filter for removing certain types of substances from a liquid or gaseous fluid (in particular for retaining metal ions). DESCRIPTION OF THE FIGURES FIGS. 1 to 4 illustrate the invention.
[0008] FIG. 1 shows a micrograph obtained by light microscopy of a polyurethane open porosity cellular foam used in the process according to the invention, the cell size of which is about 4.433 ± 0.362 mm; window size of about 2,423 ± 0,341 mm; and bridge diameter of about 0.460 ± 0.047 mm. The length of the white bar at the top right indicates 5 mm. FIG. 2a presents results obtained by X-ray photoelectron spectroscopy of the Ois / Cis atomic ratio. measured on the surface of the unmodified and multi-state C31410 Bulpren TM polyurethane elastomeric cellular foam of the process according to the invention (control polyurethane foam C31410: diagram - after contact with the compound (b) and a single wash = bar A, after two washes = bar B, after three washes = bar C). There is an increase in the proportion of oxygen atoms between the control C31410 foam and the foams modified with the compound (b), which is a control indicator for the adhesion of polydopamine (here called PDA) (compound (b)). After 1, 2 or 3 successive washes, the ratio Ois / Cis remains unchanged, reflecting the robustness of the modification. Figure 2b shows results obtained by X-ray photoelectron spectroscopy of the Ois / Cis atomic ratio. measured on the surface of the unmodified and multi-state Foampartner® polyurethane elastomeric foam of the type 8FM2 of the process according to the invention (Control polyurethane foam 8FM2: - after contact with the compound (b) ) and a single wash = bar A, after two washes = bar B, after three washes = bar C). The increase in the proportion of oxygen atoms relative to that of carbon atoms between the control 8FM2 foam and the foams modified with the compound (b), testifies to the grafting of the PDA (compound (b)). This grafting is robust with respect to the non-variation of the ratio Ois / Cis measured after 1, 2 or 3 washing steps; cf. bars A, B and C respectively. FIGS. 3a, 3b, 3c show micrographs obtained by scanning electron microscopy (SEM) of a polyurethane elastomeric cellular foam at different stages of the process according to the invention. Figure 3a is a micrograph of the unmodified polyurethane foam type C31410 Bulpren TM from Recticel ®. The length of the white bar at the bottom right indicates 10 pm. FIG. 3b is a micrograph of the polyurethane foam shown in FIG. 3a after being placed in contact with an aqueous solution of dopamine, also called 4- (2-aminoethyl) benzene-1,2-diol (CAS: 51-61-6 ). The length of the white bar at the bottom right indicates 10 μm. Figure 3c is a micrograph of the polyurethane foam after contacting the foam obtained in Figure 3b with an aqueous solution of TiO2 nanoparticles. The length of the white bar at the bottom right indicates 1 pm.
[0009] FIG. 4 represents the evolution of the absorption spectrum of sodium 7 (AO7 or sodium 4- [(2E) -2- (2-oxonaphthhalen-1-ylidene) hydrazinyl] benzenesulfonate; CAS: 63396 5) in the presence or absence of TiO 2 nanoparticles at t = 0 and at t = 22 hours, and at t = 22 hours during a second catalytic cycle with the same reused polyurethane foam. DETAILED DESCRIPTION OF THE INVENTION Cellular (and in particular elastomeric) cellular foams (also called "alveolar" foams) used in the context of the process according to the invention are so-called "solid" foams with open porosity. Preferably it is polyurethane foams. These are commercially available in high tonnage and low cost. They are flexible and particularly resistant to mechanical and chemical stresses, while having morphological properties allowing an intimate mixing of the reagents, and thus the realization of chemical transformations under mild conditions (mainly in terms of temperature and pressure) compared to systems where the catalyst is deposited on a known type of support not being in the form of a foam with open porosity. Open-pored cellular or cellular foams are in the form of structures composed of interconnected cells randomly distributed throughout the structure of the material. As a first approximation, these cellular foams have a regular pentagonal dodecahedron type geometrical shape, and are classified according to their characteristic sizes: - "average cell size, corresponding to the equivalent diameter of the sphere inscribed in the cell; - "a" the average equivalent diameter of the opening of the pores, also called size of the "windows" or size of the "pores"; - "ds" the average equivalent diameter of the bridges, also called characteristic length of the solid skeleton, here size of the "bridges".
[0010] In one embodiment of the present invention, the open-cell modified foams according to the invention are those based on synthetic organic foam. This means that the foams of the invention are made from open cell foams that include synthetic organic materials, preferably polyurethane foams. The preparation of cellular polyurethane foams is well known to those skilled in the art. Typically, such a foam can be obtained by polymerization reaction between an isocyanate and an alcohol. The process for modifying cellular (or cellular) polymeric (in particular elastomer) foams according to the invention is a method of modifying their surface. It comprises (and preferably comprises essentially) the following two steps: a) in a first step, a cellular polymeric foam (a), preferably an open-pored polyurethane elastomeric cellular foam, is supplied, b) in a second step, said cellular polymer foam is brought into contact with at least one compound (b) chosen from compounds comprising at least one catechol unit, and preferably from catecholamines. Advantageously, said foam comprises cells of average size of between 500 μm and 5000 μm, preferably between 2000 μm and 4500 μm, and even more preferably between 2500 μm and 4500 μm. Advantageously, the average equivalent diameter of the pore opening of the cellular polymer foam is between 100 μm and 5000 μm, preferably between 1700 μm and 4500 μm. Advantageously, the average equivalent diameter of the bridges of the cellular polymeric foam is between 50 μm and 3000 μm, preferably between 200 μm and 2500 μm. By "catecholamine" is meant herein a compound having a catechol (1,2-dihydroxybenzene) nucleus, the benzene ring further having an optionally substituted ethylamine side chain. According to the invention said compound chosen from catecholamines is advantageously dopamine [4- (2-aminoethyl) benzene-1,2-diol (CAS: 51-61-6)]. Other useful compounds are, for example, norepinephrine, adrenaline and 3,4-dihydroxyphenyl-L-alanine. However, other molecules simply carrying the catechol pattern lead to a similar modification of the surface of the foamed polymeric foams. In one embodiment of the process according to the invention, at least one compound having at least one catechol unit, and preferably a compound of the catecholamine family, and even more preferentially dopamine or 4- (2-aminoethyl) benzene. -1,2-diol is supplied with aqueous solution, with an amount of between 0.05% and 10% by weight, preferably of 0.1% to 1%. The step of contacting the elastomeric cellular foam (a) and the compound (b) can be carried out by several methods. By way of example, the contact may be made by immersing the elastomeric cellular foam (a) in an aqueous solution of compound (b); impregnating an aqueous solution of compound (b) with an elastomeric cellular foam (a); or alternatively by partial or complete spraying of an aqueous solution of compound (b) on the elastomeric cellular foam (a). Advantageously, the contacting between the cellular polymer foam and the aqueous solution of compound (b), in particular by impregnation, immersion or spraying, is carried out for a period of time of between 1 and 48 hours, preferably 18 to 36 hours. and even more preferably between 20 and 30 hours. Advantageously, the contacting of the cellular polymer foam (a) and of the compound (b) is carried out in a temperature range from 0 to 100 ° C., preferably from 15 to 35 ° C., and particularly preferably from 20 to 30 ° C. In a particularly advantageous embodiment, the cellular polymeric foam (a) is contacted with an aqueous solution of compound (b) at a pH of between 5 and 10, preferably between 8 and 9. The pH of the solution can be controlled by the use of a buffer solution, for example a tris (hydroxymethyl) aminomethane hydrochloride buffer solution (Tris.HCl, CAS: 1185-53-1). Advantageously, the contacting of the cellular polymer foam (a) and the compound (b) can be carried out in aqueous solution or in a water / water-miscible organic solvent mixture. The use of water as a solvent is preferred. Several routes of functionalization of surface-modified cellular polymeric foams by the process of transforming cellular polymeric foams according to the invention have been envisaged and tested, in particular with a view to their use as a catalyst support. To do this, the process according to the invention comprises an additional step c) of functionalizing the catalyst support by deposition of a phase of at least one catalytically active material (c). In one embodiment of the method of functionalization of the catalyst support according to the invention, the functionalization of the support is carried out by grafting a catalyst 30 in the form of a metal complex, in particular a metal complex comprising at least one group capable of forming covalent bonds with the catechol structural element; said group may be, for example, an alkoxysilane group, a halosilane group (such as a chlorosilane group), an amine group or a thiol group, and the reactions leading to the formation of covalent bonds may be, for example, condensation reactions with hydroxyl functions 3024147 9 of the catechol structural element, reactions leading to the formation of imines, 1,4-type additions. or radical-type reactions, said grafting of a metal complex makes it possible to obtain a homogeneous supported catalyst also called heterogeneous single-site catalyst. Advantageously, the metal complexes (comprising at least one group capable of forming covalent bonds with the catechol structural element) used in the context of the functionalization process according to the invention are chosen from organometallic molecules or coordination compounds, and more particularly among those comprising at least one transition metal.
[0011] In one embodiment of the method of functionalizing the catalyst support according to the invention, the functionalization of the support is carried out by non-covalent grafting of the catalyst in the form of metal particles, which are advantageously metal nanoparticles. The grafting of the metal particles on the surface of the support is effective by the presence of catechol groups. There is thus a support of heterogeneous catalysts. Advantageously, the metal particles used in the context of the functionalization process according to the invention are chosen from those of Ag, Fe, Co, Ni, Ru, Rh, Pd, Ir, Pt, Au, Ce, and those of the associated mixed oxides. to these elements, for example, Fe2O3, NiO2, Ni2O3, CeO2, as well as among those of other oxides such as TiO2, ZnO, WO3, SnO2, and any possible combinations of these nanoparticles.
[0012] Advantageously, the metal nanoparticles used in the context of the process according to the invention have an average particle size of between 0.5 and 100 nm, preferably 0.5 and 20 nm, and even more preferentially between 0.5 and 15 nm. nm. Consideration of the size of the catalytic nano-objects used may depend on their composition, and in particular on their metallic or oxide character: the surface properties are strongly linked to the size of the metallic nanoparticles (gold and ruthenium) for example), less strongly in the case of oxides (TiO2). Preferably, the step of functionalizing the catalyst support is carried out by deposition of the active phase according to at least one of the following techniques: by impregnation, by aerosol, or by droplets; - by chemical vapor deposition; - by capillary impregnation. Advantageously, the step of functionalizing the catalyst support is carried out at a temperature of between 5 and 80 ° C., preferably between 15 and 60 ° C., and even more preferably between 15 and 50 ° C.
[0013] The invention provides significant improvements over heterogeneous catalysts supported on rigid cellular foams, e.g., carbon foams, silicon carbide foams, metal foams, or alumina foams. Indeed, polyurethane foams, which are elastomeric foams, have great flexibility and impact resistance compared to metal foams or ceramics typically used. In addition, the active phases of the cellular foams obtained by the process according to the invention can be easily recovered, for example by simple combustion of cellular foams, which is a significant advantage, especially when the materials used as active phase are very expensive. For metal or ceramic cellular foams according to the state of the art, the recovery of the active phase requires complex chemical treatments and pollutants. A particularity of the catalysis supports according to the invention is related to the choice of compound (b) which is chosen from compounds having at least one catechol unit, and preferably from catecholamines. Indeed, the main disadvantage of polymeric foams for use as a catalyst support is their low temperature resistance: it is not possible to subject the active phase precursors (for example metal oxides) deposited on these supports. the same activation treatments (typically: reduction under hydrogen) as when they are deposited on a metal or ceramic foam because this reaction requires a temperature which may degrade the polymer foam. This is one of the main reasons why open-pored cellular polymeric foams have not been used as a catalyst support (the other reason being the poor adhesion of active phase precursors or active phases due to smoothness of the surface of the bridges that form the foam). The inventors have found that the modification of the surface of the cellular polymeric foams according to the invention by a compound having at least one catechol unit, and preferentially chosen from catecholamines (such as dopamine), makes it possible to overcome these two difficulties at the same time. . In particular, it is possible to overcome the phase of reduction of the active phase precursor deposited on said polymer foam because the catecholamines act as a reducing agent; this effect is more pronounced when said active phase precursor is deposited in the form of nanoparticles. Moreover, the presence of a compound having at least one catechol unit, and in particular the presence of a catecholamine, stabilizes the nanoparticles in their chemical integrity, particularly with respect to the oxidizing action of the air which can degrade or deactivate the nanoparticles.
[0014] Furthermore, when the modified cellular polymer foam obtainable by the process according to the invention is used as a supported homogeneous catalyst (which is impossible with metal or ceramic foams which can only serve as carrier materials). heterogeneous catalysts), the separation of the products and of the catalyst 5 is greatly facilitated with respect to the unsupported homogeneous catalysts used in particular in fine chemistry or in hydroformylation reactions, which allows the industrial scale up for reactions for which it would have been unthinkable to use them in homogeneous conditions, due in particular to the difficulty of separating the homogeneous catalyst from the products of the reaction. Indeed, in some areas of chemistry, such as pharmaceutical chemistry, the level of residual metal (from the catalyst) in the product obtained by catalysis should not exceed a threshold which is at a very low level. The method according to the invention allows catalytic reactions under conditions of temperature and pressure "softer" than in a traditional reactor (batch reactor, semi-continuous or closed, called "batch reactor") thanks to the properties of material transfer of the foam, especially in the case of biphasic reactions (gas / liquid), such as hydrogenation or hydroformylation. Thus, the modified cellular foams obtainable by the process according to the invention have many advantages over rigid metal or ceramic foams currently used as a catalyst support in the chemical, pharmaceutical and / or pharmaceutical industry. or cosmetic. Indeed, rigid metal foams or ceramics have a number of limitations. In particular, they lack flexibility: the metal foams or ceramics conventionally used are very brittle. On the other hand, the choice of types of catalysts that can be supported is limited to surface-adsorbed metal (nano) particles, hence to heterogeneous catalysts only. In addition, the catalysts deposited on these known supports are not very durable, their aging is mainly due to the desorption and oxidation of the metal species on the foam. And finally, rigid metal foams or ceramics are quite expensive.
[0015] The open-pored cellular foams obtainable by the process according to the invention can be used directly (ie after modification with the compound (b)) or after the deposition of other phases (c '). that is, after a further functionalization step c)), as a selective filter for selectively removing certain types of substances from a liquid or gaseous fluid. For example, metal ions of water, such as iron ions, can be selectively removed.
[0016] The cellular polymer foams modified according to the invention by contacting with at least one compound chosen from catecholamines may undergo other chemical functionalizations, for example by the covalent grafting of compounds comprising silane groups, amine groups or thiol groups. This further broadens the spectrum of surface properties that can be imparted by the process according to the invention to cellular polymeric foams. Examples The invention is illustrated above by seven examples which, however, do not limit the invention. Example 1 relates to contacting a polyurethane cellular foam with an aqueous solution of dopamine. Example 2 relates to the functionalization of the cellular foam obtained in Example 1 with an aqueous solution of fluoresceinamine.
[0017] Example 3 relates to the functionalization of the cellular foam obtained in Example 1 with an aqueous suspension of TiO 2 titanium dioxide nanoparticles. Example 4 relates to the functionalization of the cellular foam obtained in Example 1 with an aqueous suspension of ruthenium nanoparticles (Ru (0)). Example 5 relates to the photocatalysis of orange acid 7 using the functionalized cellular foam obtained in Example 3. Example 6 relates to hydrogenation tests of styrene using the functionalized cellular foam obtained as Example 4 Example 7 relates to the functionalization of a dopamine-modified polyurethane cellular foam, Michael addition-1,4 of a thiol or Schiff base reaction (and / or by Michael addition-1,4) of an amine. In these examples, certain abbreviations have been used: PU: Polyurethane foam PDA: Polydopamine PU-PDA: Polyurethane foam comprising on its surface an intermediate phase of polydopamine. Ru: Ruthenium PU-PDA-Fluo: Polyurethane foam comprising an intermediate phase of polydopamine and an upper phase consisting of fluoresceinamine.
[0018] PU-PDA-Ru (0): Polyurethane foam comprising an intermediate phase of polydopamine and a catalytic active phase consisting of ruthenium nanoparticles.
[0019] PU-PDA-TiO 2: Polyurethane foam comprising an intermediate phase of polydopamine and a catalytic active phase consisting of titanium dioxide nanoparticles. your. Example 1: Typical procedure for grafting polydopamine (PDA) onto the polyurethane (PU) foam surface to obtain a PU-PDA foam In Example 1, a filter for removing certain types of a liquid or gaseous fluid or a polyvalent carrier for heterogeneous catalysts or supported homogeneous catalysts has been obtained by contacting a polyurethane elastomeric cellular foam with a dopamine solution, which process corresponds to reaction scheme 1 below: Reaction 1: Preparation of a Filter or a Catalytic Support Dopamine (2 mg / ml) PU PU-PDA TRIS.HCl 10 mM, pH 8.5 ta, 24h In a stirred solution of 4- (2-aminoethyl) hydrochloride 1,2-benzenediol (CAS: 62-31-7, also called dopamine hydrochloride), prepared by dissolving dopamine hydrochloride (2 mg / mL) in an aqueous solution (60 mL) of tris (hydroxymethyl) aminomethane (sometimes called "Tris"; CAS 77-86-1) at a molar concentration of 10 mM whose pH is adjusted to 8.5 by dropwise addition of a 1M aqueous HCl solution, is immersed a sample of polyurethane foam C31410 Bulpren TM from the company Recticel or 8FM2 Foampartner company size 2x2x2 cm3 and mass between 200 and 250 mg. The reaction mixture is stirred at room temperature for 24 hours. The process of polymerizing dopamine to polydopamine is characterized by changing the color of the reaction medium to dark brown. The polyurethane foam grafted with polydopamine (PU-PDA) is then rinsed with ultrapure water (MiliQ) and then stirred in 50 mL of MiliQ water for 10 min. The washing procedure is repeated 5 times. The persistent brownish color on the surface of the foam is characteristic of the effective grafting of the PDA. The product obtained is dried by compressed air flow and then in an oven (60-70 ° C) overnight.
[0020] Analyzes of the foam surface obtained by X-ray photoelectron spectroscopy (XPS) confirm the adsorption of polydopamine on the surface of the polyurethane foam C31410 Bulpren TM from Recticel and 8FM2 from Recticel. Foampartner company (see Figures 2a and 2b). The significant increase in the atomic ratio 0 (1s) / C (1s) measured by XPS between unmodified and modified elastomeric foams demonstrates the presence of PDA and its resistance to washing. In addition, scanning electron microscopy (SEM) analyzes confirm the presence of PDAs on the surface of the Recticel C31410 Bulpren TM foam (see Figures 3a and 3b). Example 2: Typical procedure for the grafting of fluoresceinamine on the surface of polyurethane foam functionalized with polydopamine (PU-PDA) In this example, the PU-PDA foam obtained in Example 1 was functionalized with an aqueous solution of fluoresceinamine to form a fluorescent compound called PU-PDA-Fluo. This example is intended in particular to demonstrate that polydopamine can be functionalized by reaction with an amine group (by Schiff base reaction and / or Michael addition-1,4), which makes it possible to envisage functionalization. PU-PDA with any molecule having an amine group including metal complexes. This fluorescent compound makes it possible to easily visualize the functionalization of the polydopamine layer formed on the surface of the polyurethane foam by fluorescence optical microscopy techniques. To a stirred solution of 5-aminofluorescein (CAS: 3326-34-9, also referred to as fluoresceinamine, isomer I), prepared by dilution of 5-aminofluorescein (0.5 mg / mL) in an aqueous solution of Tris-HCl to 10 mM (pH 8.5, 60 mL) prepared according to Example 1, is immersed the PU-PDA foam prepared according to Example 1. The reaction mixture is stirred and heated at 60 ° C for 3 hours, then stirred at room temperature for 16 hours. The PU-PDA foam grafted with fluoresceinamine (PU-PDA-fluoresceinamine) is then rinsed with ultrapure water (MiliQ) and then stirred in 50 mL of MiliQ water for 10 min. The washing procedure is repeated 3 times. The PU-PDA-Fluo foam thus obtained is dried by compressed air flow and then kept at ambient temperature. Analysis by fluorescence microscopy (excitation at 365 nm) confirms the presence of fluoresceinamine on the PU-PDA-Fluo foam surface; the layer is continuous and homogeneous. The fluorescence intensity (measured with Image software) on a given surface is twice as high when the PU-PDA foam is modified by fluoresceinamine, relative to the same unmodified foam. In addition, the presence of fluoresceinamine on the PU-PDA-Fluo foam surface has also been demonstrated by XPS. A 34% decrease in the atomic ratio 3024147 15 (1s) / C (1s) and 14% of the ratio N (1s) / C (1s) between the PU-PDA foam and the PUPDA-Fluo foam attests to the grafting of the amino derivative. A similar experiment was carried out with Foampartner ® 8FM2 polyurethane foam, with a similar result.
[0021] Example 3: Typical procedure for grafting TiO 2 nanoparticles onto the surface of polyurethane foam functionalized with polydopamine (PU-PDA) In this example, the PU-PDA foam obtained in Example 1 was functionalized with a suspension in an aqueous medium of metal nanoparticles of titanium dioxide to form a catalyst called PU-PDA-TiO 2.
[0022] To 10 mM Tris.HCl aqueous solution (pH 8.5, 50 ml) prepared according to Example 1 was added 1 gram of a commercial nanopowder TiO 2 (anatase type and particle size of about 15 nm). After being stirred overnight at 1000 rpm using a magnetic stirrer, the TiO 2 suspension is sonicated for 30 minutes in a water bath (25 ° C) to obtain a well dispersed suspension of nanoparticles. TiO2. In this slurry of TiO 2 nanoparticles is immersed the PU-PDA foam prepared according to Example 1, then the reaction mixture is stirred at about 1000 rpm and heated at 40 ° C for 3 hours. The PU-PDA foam grafted with the TiO 2 nanoparticles (PU-PDA-TiO 2) is then rinsed with MiliQ ultrapure water and then stirred in 50 ml of MiliQ water for 10 min.
[0023] The washing procedure is repeated 5 times. The product obtained (PU-PDA-TiO 2) is dried by compressed air flow and then in an oven (60-70 ° C) overnight. The photoelectron spectrometry (% Ti2p /% Cls = 0.09871) and scanning electron microscopy (SEM) analyzes confirm the presence of TiO 2 nanoparticles on the PU-PDA foam surface (see FIG. 3c).
[0024] Example 4: Typical procedure for grafting Ru (0) nanoparticles onto the surface of polyurethane foam functionalized with polydopamine (PU-PDA) In this example, the PU-PDA foam obtained in Example 1 was functionalized with an aqueous suspension of ruthenium metal nanoparticles to form a catalyst called PU-PDA-Ru (0). The reaction scheme of the preparation of this foam is shown below: Reaction Scheme 2: Preparation of 0.1 M NaBH4 Ruthenium Nanoparticle Catalyst RUCI3.31-120, pH <4.9 H 2 O Dopamine (2mg / mL) Ru (0) PU PU-PDA ".- PU-PDA-Ru (0) TRIS-HCl 10mM, pH 8.5 ta, 24 hr, 24h and then wash with water (x5) To an aqueous solution (50 mL) of RuC13.3H2O (26.1 mg, 0.1 mM) was added dropwise a freshly prepared aqueous solution (1.8 mL) of 0.1 NaBH4. M with vigorous stirring and at room temperature. The reduction process occurs rapidly and is characterized by gradual change of color; dark brown to light brown then green-brown and finally dark brown again. The addition of NaBH4 is complete when the reaction medium is dark brown again (pH <4.9). The colloidal solution is then stirred overnight at room temperature to obtain a well dispersed suspension of ruthenium nanoparticles (0), particle size between 1 and 2 nm. In this suspension of ruthenium nanoparticles is immersed the PUPDA foam prepared according to Example 1, then the reaction mixture is stirred at room temperature for 24 hours. The PU-PDA foam grafted with the ruthenium (0) nanoparticles (PU-PDA-Ru (0)) is then rinsed with MiliQ water and then stirred in 50 ml of MiliQ water for 10 min. The washing procedure is repeated 5 times. PU-PDARu (0) is dried by compressed air flow, then in an oven (60-70 ° C) overnight. Example 5 Photocatalysis of Orange Acid 7 Using PU-PDA-TiO2 as Catalyst In this example, a photocatalyst test of orange acid 7 (AO7) was performed using the PU-PDA-TiO2 cell foam obtained in Example 3. The reaction scheme is shown below: Reaction Scheme 3: Photocatalysis of Orange Acid A07 SO3Na SO3Na PU-PDA-TiO2 OH CO2H OH UVA (6W +4 N), Visible ( 100 μA), water, ta, t (h) azo hydrazone = 430 nm = 485 nm = 310 nm 2 = 228 nm colorless orange In an aqueous solution (50 mL) of 4- (2-hydroxy-1-naphthylazo) sodium benzenesulfonate (CAS: 633-96-5, commonly referred to as orange acid 7 or AO7) at a concentration of 2.7 × 10 -E M (pH = 5.4) placed in a 100 mL beaker, are immersed in four samples. of PU-PDA-TiO2 foams (previously prepared according to Example 3, and of size = 0.5 × 2 × 2 cm 3). The solution is stirred at 250 rpm using a magnetic stirrer in the dark for 30 minutes to equilibrate, then irradiated with 3 lamps (1 visible lamp at 100 W placed above, and 2 UVA lamps (λmax = 365 nm). ) respectively at 6 W and 4 W, placed on the sides). The reaction medium is stirred for 22 hours. The catalytic conversion of AO7 is characterized by the discoloration of the solution and is followed by UV-visible spectrophotometry (see UV spectra Figure 4). This catalytic conversion is complete in 22 hours, and the foams can be reused at least once after washing with ultrapure water (MiliQ) without loss of activity. Example 6 Hydrogenation of Styrene Using PU-PDA-Ru (O) as Catalyst In this example, the hydrogenation of styrene 1 to ethylbenzene 2 was carried out using the PU-PDA-Ru (0) cellular foam obtained from Example 4. The reaction scheme is shown below: Reaction Scheme 4: Hydrogenation of styrene PU-PDA-Ru (O) H 2 (60mMu), 450 (rev / min) 70 ° C, EtOH, t (h) According to the state of the art, this reaction can form a by-product of ethylcyclohexane 3. The hydrogenation of styrene 1 is carried out in a glass tetra-neck reactor (250 ml) equipped with a condenser. The PU-PDA-Ru (0) foam is attached to the end of the mechanical stirrer in a perforated glass cage. The catalyst is immersed in a solution of styrene (0.23 mL, 0.02M) in ethanol (100 mL). The reaction medium is heated to 70 ° C. with mechanical stirring (approximately 450 rpm) and the hydrogen is continuously bubbled in the solution with a flow rate of 60 ml / min. 0.5 ml of the reaction medium are taken after 6 and 22 hours of reaction and analyzed by gas phase chromatography to determine the conversion. After 6 hours of reaction, 4% of ethylbenzene 2 is obtained; after 22 hours of reaction, 7% of ethylbenzene 2 is obtained. The quantity of ethylcyclohexane 3 formed was negligible, which underlines the selectivity of the reaction with this catalytic system. This example also demonstrates that in the case of the use of dopamine as compound (b) in the process according to the invention, it is possible to dispense with the step of reducing the active phase (Ru). This step is necessary or even essential in the case of systems according to the state of the art where the catalyst is deposited on a support of ceramic, carbon or metal type. EXAMPLE 7 Functionalization of PU-PDA Foams by Grafting a Thiol or an Amine On a Polyurethane Foam C31410 Bulpren TM from Recticel Company Modified with Polydopamine (PU-PDA), HS- (CH2) was grafted. ) 2-COOH via the Michael addition-1,4 of the thiol function on the aromatic ring of the PDA. For this purpose HS- (CH 2) 2 -COOH was used at 0.5 mg / ml in an aqueous solution of NaOH (0.1M) at room temperature. The presence of the thiol on the modified PU-PDA foam has been demonstrated by XPS. The significant increase in the S (2p) / C (1s) atomic ratio measured by XPS between the unmodified PU-PDA foam and the modified PU-PDA foam attests to the presence of the thiol. The same experiment was made with Foampartner 8FM2 polyurethane foam with a similar result.
[0025] In a further experiment, a C31410 Bulpren TM polyurethane foam from the company Recticel modified with polydopamine (PU-PDA) of NH 2 - (CH 2) 6 -NH 2 was grafted via a Schiff base reaction (and / or a Michael addition-1,4). For this, NH 2 - (CH 2) 6 -NH 2 was used under the following conditions: at a rate of 0.5 mg / ml in an aqueous solution of Tris (15 mM) at pH 8.6 at 60 ° C. for 3 h, followed by 16 h at rt The presence of the amine on the PU-PDA foam thus modified was demonstrated by XPS. The 14% decrease in the 0 (1s) / C (1s) atomic ratio and the 63% increase in the N (1s) / C (1s) atomic ratio measured by XPS between the unmodified PU-PDA foam and the the modified PU-PDA foam testifies to the presence of the amine. A similar experiment was performed with Foampartner ® 8FM2 polyurethane foam with a similar result.
权利要求:
Claims (12)
[0001]
REVENDICATIONS1. A method of modifying an open porosity cellular polymeric foam, preferably polyurethane, comprising the steps of: a) supplying an open porosity cellular polymer foam (a); b) said cellular polymer foam is brought into contact with at least one compound (b) chosen from compounds comprising at least one catechol unit, and preferably from catecholamines, to obtain a cellular polymeric foam comprising on its surface an intermediate phase formed from said compound having at least one catechol pattern.
[0002]
2. Method according to claim 1, characterized in that the step of contacting said cellular polymer foam (a) and the compound (b) is carried out among one of the following techniques: i) immersion of said polymer foam cell (a) in an aqueous solution of compound (b); ii) impregnating an aqueous solution of compound (b) with said cellular polymeric foam (a); iii) partially or completely spraying an aqueous solution of compound (b) on said cellular polymeric foam (a).
[0003]
3. Method according to claim 1 or 2, characterized in that the cellular polymer foam (a) comprises cells of average size of between 500 μm and 5000 μm, preferably between 2000 μm and 4500 μm, and even more preferentially between 2500 μm. pm and 4500 pm.
[0004]
4. Process according to any one of claims 1 to 3, characterized in that the compound (b) advantageously chosen from catecholamines is 4- (2-aminoethyl) benzene-1,2-diol, or a derivative thereof. -this.
[0005]
5. Method according to any one of claims 1 to 4, further comprising a step c) of functionalization of said cellular polymer foam by deposition of a phase of at least one material (c) catalytically active or catalytic phase precursor active, said at least one material (c) being selected from the group consisting of: metal complexes having at least one group capable of forming covalent bonds with the catechol structural element, for example a trialkoxysilane group, an amine group or a thiol group, and more particularly the coordination compounds or organometallic molecules of the transition metals. the metal nanoparticles, preferably the metal nanoparticles chosen from those of Ag, Fe, Co, Ni, Ru, Rh, Pd, Ir, Pt, Au, Ce, or those of the mixed oxides associated with these elements, such as Fe2O3 , NiO 2, Ni 2 O 3, CeO 2, as well as among those of other oxides, such as TiO 2, ZnO, WO 3, SnO 2, or any possible combinations of these nanoparticles. 10
[0006]
6. Method according to claim 5, characterized in that the metal nanoparticles have an average particle size of between 0.5 and 100 nm, preferably between 0.5 and 20 nm, and even more preferentially between 0.5 and 15 nm. nm. 15
[0007]
7. Method according to claim 5 or 6, characterized in that the catalytically active phase or catalytically active phase precursor is deposited by at least one of the following techniques: - by impregnation, aerosol, or by droplets; - by chemical vapor deposition; By capillary impregnation.
[0008]
8. Method according to claim any one of claims 5 to 7, characterized in that the functionalization step is carried out at a temperature between 5 and 80 ° C, preferably between 15 and 60 ° C, and even more Preferably between 15 and 50 ° C,
[0009]
An open porosity functionalized polymeric cellular foam obtainable by the process of any one of claims 1 to 8.
[0010]
10. Use of an open porosity cellular polymer foam obtainable by the process according to any one of claims 1 to 4 as a catalyst support or as a filter.
[0011]
11. Use of an open porosity functionalized polymeric cellular foam obtainable by the process of any one of claims 5 to 8 as a catalyst, and more particularly as a supported and / or heterogeneous homogeneous catalyst. 3024147 22
[0012]
12. Use of an open porosity functionalized polymeric cellular foam obtainable by the method of any one of claims 1 to 8 as a selective filter for removing certain types of substances from a liquid or gaseous fluid. 5
类似技术:
公开号 | 公开日 | 专利标题
FR3024147A1|2016-01-29|METHOD FOR MODIFYING THE SURFACE PROPERTIES OF ELASTOMERIC CELLULAR FOAMS
EP1069950B1|2001-12-12|Photocatalytic composition
Xu et al.2018|Nitrogen–doped GO/TiO2 nanocomposite ultrafiltration membranes for improved photocatalytic performance
Li et al.2015|Influence of Ag/TiO2 nanoparticle on the surface hydrophilicity and visible-light response activity of polyvinylidene fluoride membrane
US9486747B2|2016-11-08|Nanocomposite membranes with advanced antifouling properties under visible light irradiation
EP2925431B1|2019-02-27|Method for preparing an optionally functionalised glass having bimodal porosity, and said glass
Choi et al.2016|Ag nanoparticle/polydopamine-coated inverse opals as highly efficient catalytic membranes
Zhang et al.2018|Biocatalytic membrane based on polydopamine coating: a platform for studying immobilization mechanisms
CA2491756A1|2004-01-22|Method for preparing catalysts for heterogeneous catalysis by multiple-phase impregnation, catalysts and use of said catalysts
Sawunyama et al.1999|Photocatalysis on TiO2 surfaces investigated by atomic force microscopy: photodegradation of partial and full monolayers of stearic acid on TiO2 |
Mozia et al.2015|A study on the stability of polyethersulfone ultrafiltration membranes in a photocatalytic membrane reactor
Vijwani et al.2015|Hierarchical hybrid carbon nano-structures as robust and reusable adsorbents: Kinetic studies with model dye compound
EP1846326A1|2007-10-24|Materials based on tangled nanotubes or nanofibres, preparation method thereof and use of same
Huertas et al.2017|Sol-gel membrane modification for enhanced photocatalytic activity
Hidalgo et al.2005|Highly photoactive supported TiO2 prepared by thermal hydrolysis of TiOSO4: Optimisation of the method and comparison with other synthetic routes
CN107109086A|2017-08-29|Composition and its application including frustule
Plesch et al.2012|Zr doped anatase supported reticulated ceramic foams for photocatalytic water purification
Kumakiri et al.2011|Photocatalytic membrane contactors for water treatment
Cheng et al.2021|Rapid and robust modification of PVDF ultrafiltration membranes with enhanced permselectivity, antifouling and antibacterial performance
US9802841B2|2017-10-31|Method for treating hexavalent chromium-containing aqueous solution
Younas et al.2018|Fouling-free ultrafiltration for humic acid removal
Miranda et al.2020|Facile synthesis of an aminopropylsilane layer on Si/SiO2 substrates using ethanol as APTES solvent
EP2470299B1|2014-07-09|Catalyst for the photocalytic treatment of gaseous media including carbon monoxide
WO2017064418A1|2017-04-20|Metal nanoparticles supported on a glass-foam substrate and uses for the catalysis of chemical reactions
Mishra et al.2020|Polydopamine mediated in situ synthesis of highly dispersed Gold nanoparticles for continuous flow catalysis and environmental remediation
同族专利:
公开号 | 公开日
EP3172266A2|2017-05-31|
FR3024147B1|2018-04-20|
CN106795317A|2017-05-31|
WO2016012689A2|2016-01-28|
US20170210872A1|2017-07-27|
WO2016012689A3|2016-03-17|
US11267947B2|2022-03-08|
引用文献:
公开号 | 申请日 | 公开日 | 申请人 | 专利标题
CN103613780A|2013-11-14|2014-03-05|中国科学院化学研究所|Method for surface modification of hydrophobic polymer microporous membrane|
US20080178738A1|2007-01-29|2008-07-31|Foamex L.P.|Absorbent and/or filter materials comprising open cell foams coated with photocatalytic titanium dioxide, and methods of making and using the same|
FR2935909B1|2008-09-12|2011-01-14|Centre Nat Rech Scient|PHOTOCATALYSTS BASED ON THREE-DIMENSIONAL FOAMS STRUCTURED OF CARBON OR CARBON MATERIAL|
CN103566776B|2013-11-06|2015-06-17|复旦大学|Photocatalytic inorganic nanoparticle/polydopamine/polymer self-cleaning composite film and preparation method thereof|US20190321522A1|2016-06-17|2019-10-24|Cornell University|Foam actuators|
FR3054237B1|2016-07-25|2020-06-12|Centre National De La Recherche Scientifique - Cnrs|REDUCTION KIT, REDUCING COMPOSITION AND THEIR USE|
CN107057326A|2017-02-16|2017-08-18|四川大学|Composite of photoresponse shape memory selfreparing and preparation method thereof, restorative procedure and application|
CN108148221A|2017-12-29|2018-06-12|深圳大学|A kind of flexible porous substrate of metal nanoparticle modification and preparation method thereof|
法律状态:
2015-07-29| PLFP| Fee payment|Year of fee payment: 2 |
2016-01-29| PLSC| Publication of the preliminary search report|Effective date: 20160129 |
2016-10-24| PLFP| Fee payment|Year of fee payment: 3 |
2017-07-12| PLFP| Fee payment|Year of fee payment: 4 |
2018-07-24| PLFP| Fee payment|Year of fee payment: 5 |
2019-07-31| PLFP| Fee payment|Year of fee payment: 6 |
2020-07-31| PLFP| Fee payment|Year of fee payment: 7 |
2021-07-29| PLFP| Fee payment|Year of fee payment: 8 |
优先权:
申请号 | 申请日 | 专利标题
FR1457055A|FR3024147B1|2014-07-22|2014-07-22|METHOD FOR MODIFYING THE SURFACE PROPERTIES OF ELASTOMERIC CELLULAR FOAMS|
FR1457055|2014-07-22|FR1457055A| FR3024147B1|2014-07-22|2014-07-22|METHOD FOR MODIFYING THE SURFACE PROPERTIES OF ELASTOMERIC CELLULAR FOAMS|
EP15759503.4A| EP3172266A2|2014-07-22|2015-07-09|Method for modifying the surface properties of elastomer cellular foams|
CN201580039797.9A| CN106795317A|2014-07-22|2015-07-09|For the method for the surface characteristic of modified elastomer cell foams|
PCT/FR2015/051903| WO2016012689A2|2014-07-22|2015-07-09|Method for modifying the surface properties of elastomer cellular foams|
US15/326,539| US11267947B2|2014-07-22|2015-07-09|Method for modifying the surface properties of elastomer cellular foams|
[返回顶部]